Gutenberg · e01.org
Cover of The Silversmith's Handbook
Project Gutenberg cover, or a typographic cover where none is held.

Gutenberg · ebook 47816

The Silversmith's Handbook

by George E. Gee · English · public domain in the US

  • Language English
  • PG edition 2014
  • Rights public domain (US)
  • Source Project Gutenberg
0%

Contents

    The Silversmith's Handbook by George E. Gee is an English public-domain text held from Project Gutenberg (ebook #47816). Emphasized text is displayed as _Italic_. Except in tables where the characters ¼ and ½ were used, whole and fractional numbers are shown like: 36-1/8.

    PREFACE TO THE FOURTH EDITION.

    In issuing the present edition, a few introductory remarks are necessary to explain that numerous revisions have been made in Chapters VI. and VII. (by means of the Tables referred to below) regarding the cost prices of the different alloys, solders, etc., which I trust will increase the value of the book.

    Through the repeal of the silver duty in the year 1890, a great impetus has been given to the Silver industry of this country, and notwithstanding the length of time that has elapsed since this book was first published, a steady demand has continued for its possession by workers in the precious metal trades--a fact which is gratifying to the Author, not only because a reprint is again called for, but as showing that the work has held its position, and may now justly claim to be a standard authority on the subject of which it treats.

    It has not been found necessary to interfere with the general processes embodied in the book, as they are practically the same as formerly; but as regards the commercial value of silver, there is again a considerable depreciation[A] to record on the prices prepared for the second edition in 1885, and it becomes imperative that this depreciation should be dealt with in this new edition, in order to bring the work up to date.

    [A]

    s. d.
    In 1877 fine silver cost 5 2 per ounce.
    " 1885 " " 4 8 "
    " 1906 " " 3 0 "

    The market price of silver has for many years been of a very variable nature, almost each day's prices showing a difference, so that it would be impossible to provide the reader with an unvarying fixed price per ounce. The best and most practical thing to do under the circumstances, it seemed, was to carefully revise the different cost prices of the alloys and solders specified in Chapters VI. and VII. and give them by way of approximate Tables, compiled for each chapter separately. These two Tables follow this Preface (making pp. ix. and x.) and will serve as a ready reference for present workers in the silver trades.

    Thus, by bringing the figures down to date, the work may still retain its reliable character as a practical guide to the silversmith's workshop.

    G. E. GEE.

    58, Tenby St. North, Birmingham.
    January, 1907.

    PUBLISHERS' NOTE TO FIFTH EDITION.

    In February 1921 silver was quoted at 34-1/2_d._ to 36-1/8_d._, and it is therefore sufficient to note that the prices at that date correspond approximately to those current in 1907. It should be noted that the melting of British gold and silver is prohibited, as well as their export.

    Table of Revised and Up-to-date Cost Prices of the Different Alloys in

    Chapter VI.

    +-----+----------------------+-------------------+---------------------+
    |Page.| No. and quality of | Cost price 1885. | Cost price 1907 |
    | | alloy. | | and 1921. |
    +-----+----------------------+-------------------+---------------------+
    | 61 | Old standard alloy | For 4/4 per oz. | read 2/9½ per oz.|
    | 62 | New standard alloy | " 4/6 " | " 2/10½ " |
    | 64 | No. 1, silver alloy | " 4/2 " | " 2/9 " |
    | 64 | No.

    2, silver alloy | " 3/9 " | " 2/5½ " |
    | 65 | No. 3, silver alloy | " 3/6 " | " 2/3½ " |
    | 65 | No. 4, silver alloy | " 3/3 " | " 2/1½ " |
    | 66 | No. 5, silver alloy | " 3/2 " | " 2/0½ " |
    | 66 | No. 6, silver alloy | " 3/1 " | " 2/- " |
    | 67 | No. 7, silver alloy | " 3/- " | " 1/11 " |
    | 67 | No.

    8, silver alloy | " 2/10 " | " 1/10 " |
    | 70 | French coinage alloy | " 4/2 " | " 2/9 " |
    | 70 | French plate alloy | " 4/5 " | " 2/10 " |
    | 70 | French 0·800 alloy | " 3/9 " | " 2/5½ " |
    | 72 | German coinage alloy | 0·900 standard | " 2/9 " |
    | 72 | German silver wares | | |
    | | alloy | 0·950 1st standard| " 2/10¼ " |
    | 73 | Ditto | 0·800 2nd " | " 2/5½ " |
    | 73 | Ditto | 0·750 3rd " | " 2/3½ " |
    +-----+----------------------+-------------------+---------------------+

    This Table is based on the market price of fine silver being 3/- per ounce.

    Table of Revised and Up-to-date Cost Prices of the Different Solders in

    Chapter VII.

    +-----+---------------------------+-----------------+-------------------+
    |Page.| Quality of solder. |Cost price 1885. | Cost price 1907 |
    | | | | and 1921. |
    +-----+---------------------------+-----------------+-------------------+
    | 78 |Hardest silver solder |For 3/9 per oz.|read 2/5½ per oz.|
    | 79 |Hard silver solder | " 3/6 " | " 2/3½ " |
    | 79 |Easy silver solder | " 3/2 " | " 2/0½ " |
    | 81 |Best silver solder | " 3/9 " | " 2/5½ " |
    | 82 |Medium silver solder | " 3/6 " | " 2/3½ " |
    | 82 |Easy silver solder | " 3/3 " | " 2/1½ " |
    | 83 |Common silver solder | " 3/- " | " 1/11 " |
    | 84 |Enamelling silver solder | " 3/9 " | " 2/5½ " |
    | 84 | Ditto | " 3/2 " | " 2/0½ " |
    | 84 |Filigree solder | " 3/9 " | " 2/5½ " |
    | 85 |Quick-running silver solder| " 3/- " | " 1/11 " |
    | 85 |Silver solder for chains | " 3/- " | " 1/11 " |
    | 85 |Easy solder for chains | " 3/- " | " 1/11 " |
    | 85 |Common silver solder | " 2/9 " | " 1/9 " |
    | 86 |Common easy solder | " 2/9 " | " 1/9 " |
    | 86 |Arsenic silver solder | " 3/9 " | " 2/5½ " |
    | 86 | Ditto | " 3/6 " | " 2/3½ " |
    | 86 |Easy silver solder | " 3/2 " | " 2/0½ " |
    | 87 |Common easy silver solder | " 2/9 " | " 1/9 " |
    +-----+---------------------------+-----------------+-------------------+

    This Table is based on the market price of fine silver being 3/- per ounce.

    CONTENTS.

    INTRODUCTORY CHAPTER.

    Page

    Silver a Precious Metal 1
    Economy of Treatment 1
    Working Silversmiths 2
    English and Foreign Workmen 2
    Technical Education 2
    Pure Silver 3
    Plate and Ornamental Wares 4

    CHAPTER I.

    Silver.

    Silver, Characteristics of 5
    Silver for Filigree Work 5
    Indian Filigree Workers 5
    Malleability of Silver 6
    Ductility of Silver 6
    Test for Pure Silver 6
    Silver known to the Ancients 6
    Silver Currency 6
    Polished Silver 7
    Tarnishing of Silver 7
    Density of Silver 7
    Fusibility of Silver 7
    Heating Power of Silver 7
    Action of Silver under Great Heat 8
    Hardness of Silver 8
    Nitrate of Silver 8
    Silver resists Aqua-regia 8
    Chief Places of Filigree Manufacture 8
    Chief Uses of Silver 9
    Price of Silver, Commercial 9
    Ores of Silver 9
    Dissolution of Silver 9
    Caustic Alkalies 10
    Nitre 10
    Vegetable Acids 10

    CHAPTER II.

    Sources of Silver.

    Silver-mining 11
    Great Britain 11
    British Isles' Yield of Silver 11
    Spain 11
    America 11
    Native Silver 11
    European Supplies of Silver 12
    American Supply of Silver 12
    The Richest Mine 12
    State of the Jewellery Trade 12
    Yield of Silver 13
    Foreign Silver Currency 13
    Chief Sources of British Silver 13
    State in which it is found 14

    CHAPTER III.

    The Assay of Silver Ores.
    Silver and Mercury 15
    Assaying of Silver Ores 16
    Crucible Assay 16
    Fluxes for Crucible Assay 16
    Assay of Genuine Silver Ores 16
    Carbonate of Soda 16
    Dimensions of Crucible 16
    Litharge 17
    Preparation and Charge for Assay 17
    Treatment in the Furnace 18
    Casting-mould 18
    Scorification Process 18
    Fusing Cup or Scorifier 19
    Special Form of Scorifier 19
    Scorification Assay the Reverse of Crucible Assay 19
    Charge for Scorification Assay 20
    Advantages of the Process 20
    Anthracite and its Object 21
    Separation of the Silver from the Slag 21
    Borax, use of, in Assaying 22
    Continental Method of Assaying 22
    Flux and Charge for Crucible 23
    Details of the Process 23, 24
    Skittle-pot 25
    Cupellation 26
    Cupel, its Mode of Manufacture 26
    Cupel-mould 27
    Assayer's Muffle 28
    Cupel-tongs 28
    Brightening 29
    Sprouting 29
    Weighing of Silver Assay 30
    Chief Alloy of Silver 30

    CHAPTER IV.

    The Cupellation of Silver Ores.

    Test-ring 31
    Preparation of Bone-ash 32
    Defects in Bone-ash Cupel 33
    Currents of Air to the Furnace 33
    Withdrawal of the Silver from the Cupel 34
    Removal of the Litharge, Manner of 35
    Quantity of Alloy per Cupel 35
    Purity of Silver after Cupellation 37
    Ancient Method of Assaying 37
    Dr.

    Lamborn on Assaying 38
    Scriptural Testimony 37, 38
    English System of Assay 39

    CHAPTER V.

    The Alloys of Silver.

    Silversmith's Alloys 40
    Filigree Work 40
    Alloy 41
    Amalgam 41
    Metals employed in the Industrial Arts 41
    Metals, their various Characteristics 41
    Principal Alloys of Silver 42
    Copper 42
    Characteristics of Copper 43
    Protoxide of Copper 44
    Action of Acids on Copper 44
    Bean-shot Copper for Alloying 44
    Chemical name for Copper 44
    Nickel 45
    Cronstedt 45
    Density of Nickel 45
    Ductility of Nickel 45
    Malleability of Nickel 45
    Fusibility of Nickel 45
    Nickel Coinage 45
    Nickel Alloys 46
    Electro-plate 46
    Zinc 46
    Spelter 46
    Zinc in Silver Solder 46
    Annealing of Zinc 47
    Specific Gravity of Zinc 47
    Spelter used by Jewellers 47
    Tarnishing of Zinc 47
    Malleability of Zinc 48
    Ductility of Zinc 48
    Tenacity of Zinc 48
    Tin 48
    Ancient Workers in Tin 48
    Density of Tin 48
    Christianity and Tin 48
    Fusibility of Tin 48
    Dissolving of Tin 48
    Tin alloyed with Gold 49
    Tin alloyed with Silver 49
    Tin in Silversmith's Solders 49
    Vapours of Tin injurious to Gold 49
    Malleability of Tin 49
    Ductility of Tin 49
    Tenacity of Tin 49
    Scientific Name for Tin 50
    Table of Metallic Elements 50
    Melting-points of the Principal Metals 51
    Physical Properties of the Principal Metals 51

    CHAPTER VI.

    Various Qualities of Silver.

    Mechanical Uses of Silver 52
    Filigree Work 52
    Birmingham 52
    London 52
    Indian 53
    Chief Places of Filigree Manufacture 53
    Continental Cheap Labour 54
    Hand-made Articles 54
    Process of Workmanship 55
    Maltese Filigree 55
    Chinese and Japanese Filigree 56
    Filigree of Norway and Sweden 56
    Filigree working, Necessity for Pure Metal 56
    Old Method of making Filigree 57
    Twisting of the Wire 58
    Lathe, Use of 58
    Flattening of Twisted Wire for Filigree 59
    New Method of preparing Filigree Wire 59
    English Standards for Silver 60
    English Coinage 61
    Standard Silver Alloy 61
    Alloy for Hall-marking 62
    Standard Alloy of the Highest Quality 62
    Standard Alloy for Hall-marking 62
    Alloy commonly used in England 63
    Qualities used by English Silversmiths 63
    Drawbacks to Hall-marking 63
    Method of calculating the Qualities of Silver 63
    Silver Alloy No.

    1, cost 4_s._ 7_d._ per oz. 64
    " No. 1, differently calculated 64
    " No. 2, cost 4_s._ 1_d._ per oz. 64
    " No. 2, differently calculated 64
    " No. 3, cost 3_s._ 10_d._ per oz. 65
    " No. 3, differently calculated 65
    Silver Alloy No. 4, cost 3_s._ 7_d._ per oz. 65
    " No. 4, differently calculated 65
    " No. 5, cost 3_s._ 6_d._ per oz. 66
    " No. 5, differently calculated 66
    " No. 6, cost 3_s._ 3_d._ per oz.

    66
    " No. 6, differently calculated 66
    " No. 7, cost 3_s._ 2_d._ per oz. 67
    " No. 7, differently calculated 67
    " No. 8, cost 3_s._ per oz. 67
    " No.

    8, differently calculated 67
    Instructions in the Preparation of Alloys 68
    Copper for Alloying 68
    French Standards 69
    Silver Ware 69
    Coinage 69
    French Alloy for Coinage 70
    French Alloy for Plate 70
    French Alloy for Silver Ware 70
    Instructions in the Preparation of these Alloys 70
    German Standards 71
    Silver Ware 71
    Coinage 71
    Silver Alloy for the German Coinage 72
    Alloy for Plate 72
    Alloys for Silver Wares 72, 73
    Law on the Manufacture of Silver Wares 73
    Remedy allowed in Fineness 73
    Government Exports 73
    Guarantee Marks 73

    CHAPTER VII.

    Silver Solders: their Uses and Applications.

    The Act of Soldering 74
    Cause of Inferior Manufactures 74
    Tin in Solders 75
    Filed Solders 76
    Zinc in Silver Solder 76
    Solders made with Copper and Silver 76
    Hard Silver Solders 77
    Medium Solders 77
    Easy Solders 77
    Connections for Soldering 77
    Flux for Soldering 77
    Fusibility of Silver Solders 78
    Hardest Silver Solder, cost 4_s._ 1_d._ per oz.

    78
    Ditto, differently calculated 79
    Medium Silver Solder, cost 3_s._ 10_d._ per oz. 79
    Ditto, differently calculated 79
    Easy Silver Solder, cost 3_s._ 5_d._ per oz. 79
    Ditto, differently calculated 80
    Remarks on Silver Solders 80
    Composition for Solder 81
    Best Hard Solder, cost 4_s._ 1_d._ per oz. 81
    Ditto, differently calculated 81
    Medium Solder, cost 3_s._ 10_d._ per oz.

    82
    Ditto, differently calculated 82
    Easy Solder, cost 3_s._ 7_d._ per oz. 82
    Ditto, differently calculated 82
    Common Solder, cost 3_s._ 3_d._ per oz. 83
    Ditto, differently calculated 83
    Directions on the Melting of Solders 83
    Solder for Enamelling, cost 4_s._ 1_d._ per oz. 84
    " " cost 3_s._ 6_d._ per oz. 84
    Easy Solder for Filigree Work 84
    Quick Running Solder, cost 3_s._ 3_d._ per oz. 85
    Silver Solder for Chains, cost 3_s._ 3_d._ per oz.

    85
    Easy Solder for Chains, cost 3_s._ 3_d._ per oz. 85
    Common Silver Solder, cost 3_s._ per oz. 85
    Common Easy Solder, cost 3_s._ per oz. 86
    Arsenic Solder, cost 4_s._ 1_d._ per oz. 86
    Silver Solder with Arsenic, 3_s._ 10_d._ per oz. 86
    Easy Silver Solder, cost 3_s._ 6_d._ per oz. 86
    Common Easy Solder, cost 3_s._ per oz.

    87
    Another Common Solder 87
    Very Common Solder 87
    Directions in the Preparation of Solders 87
    Drossy Solders 88
    Mode of Soldering Gold and Silver 88
    Pallion Solder 88
    Blowpipes 89
    Solder-dish and Charger 89
    Soft Solder 90
    Art in Soldering 90
    Solder for Filigree 91
    Lemaille Solder 91
    English Filigree Workers 91
    Sprinkle Borax 92
    Special Soldering Flux 92
    Boiling-out Pickle 93

    CHAPTER VIII.

    On the Melting of Silver.

    Directions on Melting 94
    Weighing Metal for the Crucible 94
    Crucibles 95
    Best Crucibles to employ 95
    Fluxes: their Action on Crucibles 96
    Fluxes employed in Melting 96
    Testing the Soundness of a Crucible 97
    Mixing various Metals for melting 97
    Zinc a fusible Metal 98
    Charcoal 99
    Bad working Material 99
    Plumbago Crucible for Melting 99
    Tongs for Melting 100
    Ingot-mould 100
    Flux and the Pouring of Molten Metal 101
    Protoxide of Zinc 102
    Scrap Silver 102
    Carbonate of Soda 102
    Dissolving Impurities 103
    Lead and Tin in Silver 103
    Sal-ammoniac 103
    Lemel 103
    Mixture prepared for Crucible 104
    Burning of Lemel 104
    Skittle-pot for Lemel 104
    Melting of Lemel 105
    Another Mode of melting Lemel 106
    Crucible for Lemel 106
    Pouring of Lemel from Crucible 107

    CHAPTER IX.

    On the Working of Silver.

    Rolling Silver 108
    Annealing Silver 109
    Irregularities in Rolling-mills 110
    Messrs Kemp's Mill 110, 111
    Table of the Cost of Silver-rolling 112
    Slitting Rollers 112
    Breaking-down Rollers 112
    Wire-rolling 113
    Wire-drawing 113
    Draw-plate 114
    Draw-bench 110, 115
    Draw-tongs 115
    Drum used by Wire-drawers 115
    Fine Wire-drawing 115, 116
    Wire-drawer's Punch and Hammer 117
    Wrought Work 118
    Sparrow-hawk 119
    Raised Work 120
    Cement for Chasers 121
    Snarling-tools for Raising 122
    Art in the Silver Trade 123
    Burnished Silver Work 124
    Silver Filigree Work 125
    Stamped or Struck-up Work 126
    Press 127
    Plain Solid Work 127
    Chain Bracelets 128
    Present State of Silver Trade 128
    Silver, Liability to become tarnished 129
    Enamelling 129
    Galvanic Ring 129
    Mode of preparing Ring 129, 130
    Hollow Silver Work 131
    Stamping-press 132
    Spinning 134, 135
    Polishing 135
    Water-of-Ayr Stone 136
    Polishing-lathe 137
    Washing-out Mixture 138

    CHAPTER X.

    Enriching the Surfaces of Silver.

    Production of the best and richest Surface 139
    Oldest Method for Whitening 140
    East Indian Silversmiths 141
    Indian Mode of Whitening Silver 142
    Another Mode of Whitening 142
    Boiling-out Pan 143
    Boiling-out Mixture 143, 144
    Our Mode of Whitening 145
    Surface Refining of Silver 146
    Brown Colour on Silver Goods 146
    Common Articles of Silver 147
    Whitening Powder or Mixtures 147
    Nitrate of Silver Mixture 148
    Improving the Colour of Electro-plate 149
    Electro-plating 149
    Discoverer of Electro-plating 149, 150
    Constant Battery 150
    Best Battery for Plating 151
    Strength of Battery Solution 151
    Bunsen's Battery 152
    Exciting Mixture for Battery 152
    Zinc Amalgamation 153
    Conducting Wires 154
    Preparation of Plating Solution 155
    Cyanide Solution 156
    Black Cyanide 157
    Strength of Plating Solution 157, 158
    Inferior Plating Solution 159
    Recovery of Silver from Plating Solutions 160
    Scratch-brushing 161
    Scratch-brush Lathe 161
    Burnishing Silver Work 161, 162
    Oxidizing Silver Work 163
    Solution No 1.

    163
    Solution No 2. 164
    Solution No 3. 164
    Producing various Shades 165

    CHAPTER XI.

    Imitation Silver Alloys.

    Melting Imitation Alloys 166
    Common Silver Alloy 167
    Another 167
    Another 168
    Another 168
    Another 168
    Another 168
    Another 169
    Another 169
    Another 169
    Another 169
    Another 170
    Another 170
    Chinese Silver 170
    Imitation Silver 170
    Another 171
    Another 171
    Another 171
    Another 171
    White Alloy 172
    Clark's Patent Alloy 172
    White Alloy 172
    Alloy with Platinum 172
    Alloy with Palladium 173
    Uses for Imitation Alloys 173
    Characteristics of Imitation Alloys 174

    CHAPTER XII.

    Economical Process.

    Working Loss 175
    Lowest Estimate Real Loss 175
    Total Working Loss 176
    Shop Floors 177
    Waste-saving Precautions 177, 178
    Treatment of Waste 178
    Burning of Polishings 179
    Treatment of Waste Liquids 180
    Processes for the Recovery of Silver from Waste Waters 180, 182
    Chloride of Silver 183
    Aqua-regia 183
    Precipitating Silver in Waste Waters 183
    Solution for Precipitation 184
    Sediment in Collecting-vessels 185

    CHAPTER XIII.

    Licences and Duties.

    Acts of the Legislature 186
    43 George III., c. 69 186
    6 George I., c. 11 187
    31 George II., c. 32 188
    32 George II., c. 14 188
    24 George III., c. 53 188
    37 George III., c. 90 188
    44 George III., c. 98 189
    55 George III., c.

    185 189
    Table of Various Duties 189
    Manufactured Plate 190
    Remarks on the Licence Question 191, 196
    Act of Parliament in Licences 193
    Clause of Act 193, 194
    Tax or Licence unjustly Assessed 195, 196

    CHAPTER XIV.

    Useful Information for the Trade.

    Silversmith's Alloys 197
    Silver Wares 197
    Cleaning Plate 198
    Imitation Silver 198
    Another 198
    Removing Gold from Silver Articles 198
    Oxidizing Silver 198
    Dipping Mixture 199
    Silver Powder for Copper 199
    Powder for Silver 200
    To protect the Polish of Metals 200
    Silver-stripping Mixture 200
    Stripping Silver 201
    Soft Solder 201
    Soldering Fluid 201
    Dissolving Silver 202
    Dissolving Silver Alloy 202
    Dissolving Copper 202
    Dissolving Soft Solder 202
    Dissolving Silver Solder 202
    Dissolving Sealing-wax 202
    Resist Varnish 202
    Plate Powder 202
    Electro-plating Soft Solder 202
    Another Recipe 203
    Testing Silver Wares 203
    Another Test 204
    Perchloride of Iron 205
    Aluminium Alloy 205
    New Alloy 205
    Removing Gold from Silver Wares 205
    Silver Plating Fluid 206
    Plate-cleaning Powder 206
    Solder for Aluminium 206

    CHAPTER XV.

    Foreign Silver Standards 207
    French Work, Duty on 208
    Continental Silversmiths 209
    French Style of Work 209
    German Style of Work 210
    Indian Style of Work 210
    Austrian Style of Work 211
    English Style of Work 211
    Index 212

    THE

    SILVERSMITH'S HANDBOOK.

    INTRODUCTORY CHAPTER.

    In reviewing the rise and progress of the silversmith's beautiful and interesting art, in its relation to the manufacture of articles of personal ornament and luxury at home and abroad, we may observe at the outset, that the material of which they are composed differs widely in character from that employed by the ordinary "metalsmiths" and the manufacturer of "electro-plated wares." Silver, the material of which we are now treating, being a precious metal and of considerable value, it is essentially necessary that the most careful means be exercised in dealing with it from the commencement--that is, from the pure or fine state--and also that the utmost economy be observed in reference to the kind of mechanical treatment to which it is subjected in the production of the silversmith's work, in order to prevent too great a quantity of waste or loss of material.

    For it should be borne in mind that silver, like gold, begins to lose, in one way or another, every time it is touched; therefore, carefulness and economy will be the characteristics of our teaching, so far as regards the present subject.

    The vast majority of working silversmiths know very little of the physical and chemical properties of the metal they employ, and still less of the comparison it bears with other metals in the field of science; and this want of scientific knowledge is nowhere more apparent than in our own country, where the English workman, in art education, is much behind the foreigner; and yet we have some of the finest and best workmen, in their special branches, in the whole world.

    The English workman believes that if the work is worth doing at all, it is worth doing well; and we have no hesitation in saying, that, if a good technical education were afforded, concerning the precious metal trades, he would scarcely have an equal, and certainly no superior, abroad, in art workmanship, both in respect to the display of good taste and judgment, combined with a knowledge of design, so far as the exercise of these qualities is compatible with the manufacture of articles specially designed for use and ornament.

    The object of the information we are about to supply is to enable the practical silversmith to become a perfect master of his art or profession; and such a condition, when once achieved, will be found of considerable assistance to him in the various kinds of manufacture that present themselves; so that he will know how to begin a piece of work and when to leave it off; be able to remedy a defect in the metal when required, as well as be in a position to form an opinion as to the relative treatment of its different alloys; all of which invariably require different treatment.

    We shall commence by describing the characteristics of fine silver, carefully narrating the distinctive features of its alloys; then give an account of the processes employed, mechanical and chemical, in the silversmith's workshop; and conclude by pointing out the difference between English and foreign work in regard both to style and workmanship.

    It may be thought by the reader, if uninitiated in the art, that the costly plate and other articles made from the precious metal are manufactured from entirely pure silver, and therefore that they possess absolute freedom from alloy; but this is not the case.

    Pure silver being far too soft to stand the necessary wear and tear of (metallic) life, it is mixed with some other metal, to give it increased hardness. In the manufacture of plate and ornamental wares the metal employed is always copper, in various proportions, thus forming different commercial qualities; and of these we shall speak hereafter. Our first object is to treat of the chemical and physical properties of the pure metal.

    CHAPTER I.

    Silver.

    Pure silver is, next to gold, the finest metal, but of a smoother and more polished nature. It may be said to be almost infinitely malleable, but it will not so easily yield or extend under the hammer as fine gold. As a malleable metal, however, it stands next to it in this respect. It is characterized by its perfectly white colour, being the whitest of all the metals. It is harder than gold, yet in a pure state it is so soft that it can easily be cut with a knife. On account of its extreme softness, when in a pure state, it is employed for filigree work, being utterly devoid of that elastic power which is found in the metal when alloyed.

    It is for this reason that the Indian filigree workers, who are the finest in the world, are so very particular about the absolute purity of the metal before commencing the manufacture of their artistic work; all of which is exceedingly beautiful.

    It is reported that fine silver is capable of being beaten into leaves of less than one-hundred-thousandth part of an inch in thickness.

    For the accuracy of this statement we cannot vouch, never having had occasion to try the experiment; its employment in that form being unknown in the ordinary industrial pursuits. Fine silver is extremely ductile, and may be drawn into the very finest wire without breaking, and almost without annealing. Its purity can be partly ascertained by the latter process; for perfectly fine silver never changes colour by heat, whereas when it contains alloy it blackens if heated in contact with a current of air, and soon hardens in wire-drawing.

    Silver was a metallic element known to the ancients, and it is repeatedly mentioned in the Holy Scriptures. In the time of the patriarchs we read of it as having been constantly employed in the transactions of nations, and that it was in use as a standard of value; thus forming a circulating medium for the purpose of exchange. This function it has always continued to fulfil down to the present day, except that since the year 1816 it has not been so employed in the English currency. However, as token money, it is everywhere recognised as a circulating medium of trade. The Egyptian symbol for silver was represented by Fig.

    1, relating to the moon; in modern chemistry it is understood by ag. from the Latin name argentum, denoting silver.

    [Illustration: Luna. Fig. 1.

    Egyptian mark for Silver.]

    Fine silver is capable of receiving a polish scarcely inferior in lustre to that of highly polished steel, and in this state it reflects more light and heat than any other metal, without any perceptible change of colour for some considerable time. It is chiefly on this account, as well as its resistance to oxidation in air and water, that it is used for such a variety of purposes, not only of ornament and luxury, but also in a domestic way. Silver, unlike gold, cannot resist the influence of sulphuretted hydrogen, from the action of which it very soon becomes much tarnished if left exposed in damp rooms, &c.

    Silver ranks next to gold in point of ductility and malleability.

    When pure, its density, or specific gravity, lies between 10.47 and 10.50, taking water as 1, according to the degree of compression it has received by rolling and hammering. It is fusible at a full red heat, or about 1873° Fahr. It is a metal having a very low radiating power for heat; hence silver wire of given dimensions retains and conducts heat better than a similar piece of another metal; for the same reason, a liquid contained in a silver vessel retains its heat much longer than if placed in one made of some other substance.

    Silver volatilises when subjected to a very great temperature in the fire, emitting rather greenish fumes. It loses between 2/21sts and 3/25ths, in proportion to its impurity, of its absolute weight in air when weighed in water. In point of tenacity it occupies the fifth position among the useful metals. In hardness it lies between copper and gold; and a small addition of the former substance considerably increases this quality, in which state it is largely employed in the arts.

    Nitric acid is the proper solvent for silver, as it dissolves it with the greatest ease and rapidity, forming nitrate of silver, which is much used for medical purposes, and in art. Sulphuric and hydrochloric acids act upon it but slowly in the cold. Silver resists partially the best aqua-regia, probably on account of the dense chloride which forms on the surface of the metal, from the action of the hydrochloric acid in the mixture of aqua-regia.

    Fine silver is largely used in the industrial and commercial arts, in the manufacture of silver lace and fine filigree work; the latter branch being more commonly practised in India, Sweden, Norway, and some parts of Germany, where labour is cheap, than in England. This class of silversmith's work takes a long time to produce, and as labour forms the chief item of its cost, this, not unnaturally, acts as a great drawback in the extension of the art of very fine filigree working, in all its intricate variety, in countries where labour is dear. To this subject we shall subsequently refer again in detail.

    Fine silver, with a small proportion of alloy, is largely used by all nations for purposes of coinage. It amalgamates with nearly all the metals, but is principally used in alloys suitable to the watchmaker's and silversmith's art. The purchasable price of fine silver for manufacturing purposes, which in 1884 was 4_s._ 8_d._ is now, 1921, 3_s._ per ounce, troy weight, varying however in value according to the total amounts purchased; for which see refiners' and assayers' charge lists, to be procured at the offices of any bullion dealer.

    The silver ores of commerce have generally an intermixture of a small quantity of gold, and sometimes instances have occurred in which it has been employed in manufactures without a proper chemical investigation; and in such cases the loss resulting from the omission would have amply paid the expenses of the process.

    Exposed to the action of hot and concentrated sulphuric acid, silver dissolves, setting free sulphurous acid. By the application of this process--which is one of the most advantageous methods--silver may readily be separated from gold, sulphuric acid having no action upon the latter metal. With the exception of gold, silver perhaps more perfectly resists the action of the caustic alkalies and the powerful effects of nitre (saltpetre) than any other metal, if we omit platinum from the list of elements at present known to metallurgical chemistry.

    For reasons such as these its superiority for the manufacture of utensils for culinary and other domestic purposes is at once apparent, and because it is a metal upon which vegetable acids produce no effect.

    CHAPTER II.

    Sources of Silver.

    Strictly speaking, silver mining does not exist as a distinct operation in Great Britain, for it can hardly be said that this country possesses any great quantity of silver ore. Yet we must not disguise or leave unnoticed, in dealing with this subject, the positive fact that silver is found to some extent in our copper and lead mines, principally in the latter; but in no case, as far as we know, have mines been worked for the sake of the silver alone. It is almost always found in conjunction with lead, and it is from that source that we have a good supply of British silver.

    The average annual yield in the British Isles for some years has been equal to 800,000 ounces--a position in regard to the quantity produced ranking second only to Spain amongst the nations of the world, America, of course, being excepted. Silver is found in a native state, the commonest ore being a sulphuret.

    The chief European supplies are derived from Spain, in which country genuine silver ore exists; from Saxony and Prussia, where the ores are principally associated with lead, as in England; and from Austria, where it is for the greater part found mixed with copper. Silver is nearly always to be found in copper and lead mines, but generally in such small quantities that it is rarely worth the trouble and expense of separation.

    Considerably more than three-fourths of the whole total supply of silver comes from America; and in fact nearly the whole territory of America is said to be more or less argentiferous. Until lately Mexico carried off the palm, as containing and yielding the largest percentage of silver; but through the discovery of another mine in the United States, at Nevada, of considerable richness, which has yielded enormous supplies, we shall not be far wrong in pronouncing the silver mines in the State of Nevada to be the richest in the whole world.

    The extensive production of these mines, combined with other causes, has led to a considerable depreciation in the value of silver, and probably this may yet lead to its more extensive employment in the arts and manufactures; and, in the midst of the very general depression of the jewellery trade, any change extending in that direction would be joyfully accepted by the thousands of workmen in the precious metal trades now standing idle.

    We are told that, since the year 1860, the production of silver has increased from an average yield of eight or nine to fourteen millions per annum, or about 60 per cent.; while, on the other hand, the foreign demand for the metal (formerly largely employed for the currency) has greatly diminished.

    The rise in cost of silver during the war years and those immediately following necessitated an Act in Great Britain "to amend the law in respect of the standard fineness of silver coins current in the United Kingdom and in other parts of His Majesty's Dominions."

    The chief sources of supply in the British Isles, according to Professor George Gladstone, are as given below; and as all the silver found in this country is produced from lead ores, the average yield here given must be understood to exist in about that proportion to every ton of lead ore assayed:--Isle of Man, 50 to 60 oz.; Cornwall, about 30 oz.; Devonshire, about 30 oz.; Cardiganshire, 15 to 20 oz.;

    Montgomeryshire, 15 to 20 oz. Thus, it will be seen the lead ores of the Isle of Man yield the greatest proportion of silver in the British dominions. Silver is also found in the undermentioned counties, in all of which it is produced from lead ore:--Cumberland, Durham, and Northumberland, Denbighshire, Flintshire, and Derbyshire; but the percentage is much smaller than in the preceding cases. Ireland also yields a fair percentage of silver.

    CHAPTER III.

    The Assay of Silver Ores.

    A large proportion of the silver of commerce is extracted from ores (which are too poor to allow of their being smelted or fused) by a process called amalgamation. Founded on the ready solubility of silver, &c., in metallic mercury, the ore is first crushed to powder, then mixed with common salt, and afterwards roasted. By the adoption of this plan the silver is reduced to a state of chloride.

    The roasting is done in a reverberatory furnace, in which the heat is very gradually raised, the ore being constantly stirred; the heat is then increased sufficiently to raise the ore to a good red heat. It is then put into wooden barrels, revolving on iron axles attached to the ends, and scraps of iron are then added to it; both are then agitated together by rotary motion, the effect of which is to reduce the chloride of silver to a metallic state.

    When this is effected, it is again agitated with mercury, and a fluid amalgam is formed with the metal, together with any other metallic ingredient that may happen to be present in the roasted ore. Subsequently, to recover the silver, the mercury is driven off by heat, and the silver is thus left behind in an impure state.

    There are three ways of assaying silver ores; they are in the test assay as follows:--

    1. Melting in a crucible.
    2. Scorification.
    3. Cupellation.

    In the crucible assay the ore is commonly run down with a suitable flux, those most frequently employed being litharge, carbonate of soda, borax, and charcoal. These four substances are all that are required by the practical assayer in the treatment of the regular ores of silver.

    [Illustration: Fig. 2. Fire-clay Crucible.]

    The assaying of the genuine ores is performed in the following manner; that is, if they contain but little earthy matter. They may then be conveniently treated by fusing with carbonate of soda, on account of its cheapness, and borax, in a fire-clay crucible (Fig. 2). The dimensions of the crucible should be as follows: 4-1/2 inches in height, and 2-1/2 inches in its greatest diameter, which should be at the top. A quantity of litharge (a semi-vitrious substance, oxide of lead), more than is actually necessary to take up the whole of the silver in the ore, should be added, so as to promote fusion, and collect the ingredients into one mass at the bottom of the crucible.

    In preparing the ore for the crucible, it must be well pounded, and intimately mixed with the undermentioned chemicals:--

    Pounded silver ore 240 grains.
    Litharge 800 "
    Carbonate of soda 700 "
    Borax 300 "
    Charcoal 50 "

    Place two crucibles to warm during the time occupied in the preparation of the mixture, then put it into the warm crucible; take 100 grains more of litharge, and powder it over the contents in the vessel.

    Prepare in this manner a second mixture for the other crucible, place them both in the furnace, and put plenty of coke round them. The mixtures may be melted in an ordinary wind or melting furnace, such as is used by jewellers in the preparation of their material for art working. The fusion should take place very gradually at first, as silver in combination with lead is sensibly volatile at a high temperature: it may then be continued at a low heat for twenty-five minutes, and finally the operation may be completed with a full red heat for five minutes longer.

    During the process of fusing the contents of the crucible may be watched by removing one of the bricks from the top of the furnace, and when the whole mass has become quite liquid the crucible must be seized with a pair of suitable tongs, tapped once or twice very lightly against the side of the furnace to procure the settlement of the contents, and immediately poured into an iron mould, previously warmed and greased to prevent adhesion and spitting. Allow the mould to remain for some time, in order to partially cool, and then plunge it into a vessel of cold water.

    On cooling, the metallic elements will be found incorporated into a button, the slag can then easily be removed by tapping with a hammer on the edge, and the plunging into cold water greatly facilitates this separation. The whole mass has then to be cupelled, in order to separate the silver from the lead and other metals.

    [Illustration: Fig. 3. Fire-clay Fusing Cup.]

    Silver ores, containing a large proportion of the sulphides (chemical combinations of sulphur with metallic substances) of other metals, may be easily assayed by the scorification process, which is, without exception, applicable to the assay of all kinds of argentiferous ores; and is one of the best, most simple, and most exact methods that can possibly be employed in the extraction of silver from its ores. This process, like that of fusion with litharge, already described, has the effect of producing an alloy, and subsequently requires cupellation.

    The ore is first well pounded, and then put into a small shallow vessel made of close-grained refractory fire-clay (Fig. 3), with an excess of finely granulated lead and some borax. The fusing cup or scorifier employed in this process should be about 1-1/2 in. high and 2-1/2 ins. in its greatest diameter; some assayers, however, use them deeper in proportion to their width, and representing in form the end of an egg.

    The object of this shape is to preserve the bath of molten metal at the bottom, and that it may always be well covered and protected by the slag on the top during the process of fusing. In the scorification method the principles are exactly the reverse of those of the crucible assay; for in the latter the object is to reduce the oxide of lead to a metallic state, whereas in the former the metallic lead added to the pounded ore in the scorifier is oxidized by being fused in contact with the air. The charge for this assay may be as follows:--

    Well pounded ore 60 grains.
    Finely granulated lead 600 "
    Borax anhydrous 100 "
    Powdered anthracite 5 "

    The cups or scorifiers should be charged in the following manner: well mix the silver ore with 300 grains of granulated lead; place this mixture in a scorifier, and add 300 grs. more of granulated lead, and over the top of the whole put the burnt borax.

    The vessel may then be placed in an ordinary assay furnace or muffle, as many being introduced at one time as there is room for in the furnace, and submitted to the strongest heat for about thirty minutes; during the greater portion of this time the door should be kept closed, especially for the first fifteen minutes.

    On opening the muffle-door a current of air passes through the furnace, converting a portion of the lead into litharge; this enters into combination with the earthy portions of the ore, the other metallic sulphides, and also the borax, producing a fusible slag on the surface of the metallic bath, extending over the whole surface of the scorifier.

    The excess of lead is thus protected by this film or flux from the oxidizing effects of the currents of air admitted into the furnace, and remains united with whatever silver there may be in the ore, in a metallic state.

    The fusing should be continued longer than the thirty minutes--in fact until the slag or flux is reduced into a perfectly liquid state; stirring it well with a slender iron rod will facilitate the operation, as it will tend to mix with the mass any hard portions remaining undissolved and attached to the sides or other parts of the vessels.

    This condition of the flux is absolutely indispensable; when the slags are quite liquid, which with a strong fire will take place in from thirty to forty minutes, wrap up in a piece of paper the powdered anthracite, and drop it into the scorifier while still in the furnace or muffle. The object of adding the anthracite at the last moment is to reduce any minute portions of the metal that may exist in the slags, and remain separated from the bulk.

    When the anthracite has burnt off, which process usually takes about five minutes, this point is considered to have been attained, and the operation is then complete. The scorifier may be immediately withdrawn from the fire, and the contents poured into a suitable casting-mould, of the form represented in Fig. 4, a button of silver lead being the result.

    When cold, the metallic mass is readily separated from the slag or flux by slightly tapping with a hammer; the former may then be passed on to the next operation, viz. to be purified of its lead by the process of cupellation, which will be presently described.

    When there is not enough borax present the assayer will observe an infusible skin floating upon the surface; should this be the case more borax must at once be employed, in order to dissolve such impurity.

    When a chloride of silver ore is to be assayed, carbonate of soda must be added to the mixture to prevent sublimation.

    The following method of assaying is adopted in several large Continental establishments, where the ores have, beside the usual earthy matter and the sulphides of lead, an admixture of zinc, iron, and copper. The process is precisely similar to the crucible assay, in the case of genuine silver ores, as already described--with this exception, that no more lead is added than the ores then contain--that is, if we are treating galena or silver lead; other ores require different treatment according to their known composition.

    In this process wrought-iron crucibles are employed having the form and shape as shown in Fig. 5. They are made of thick iron plate, and are rendered secure by welding the edges firmly together. Their dimensions are as follows: a depth of 4-1/2 ins., with a thickness of iron at the bottom of 1-1/2 in., and a 1/4 of an inch in the sides; the diameter at the top of the crucible should be about 2-1/2 ins., and at the bottom between 2 and 2-1/4 ins.

    A mechanical mixture or flux is prepared to use with the ores to which we have referred, consisting of the following chemicals, all of which should be finely powdered and well mixed with the ore to be assayed:--

    Carbonate of soda 6 parts.
    Tartar 3 "
    Saltpetre 2 "
    Borax 1 part.

    The furnace used for this assay is the ordinary one, having rather a high chimney, to insure a perfect draught. In effecting the reduction of the silver, the crucible is first placed as before on the fire, and allowed to become hot; when this is accomplished, take

    Well powdered ore 480 grains.
    Prepared flux 500 "

    These ingredients should be thoroughly mixed together, and put into the red hot crucible. Fuse at a low heat for about twenty minutes, when the whole will be in a perfect state of fusion; then give about five minutes strong heat, and at the end of that time the crucible may be withdrawn, and its contents poured into an iron mould, as represented in Fig. 4, having one or two conical holes for the reception of the fused mass. The silver and lead collect at the bottom of the mould by reason of its high specific gravity.

    It may be removed by reversing the position of the latter, when a gentle tap or two will deprive it of that slag or flux which is usually attached to it. A large quantity of silver can be readily collected from its ores by an alternate use of crucibles, in which case it is possible to make a regular number of fusions per hour. Wrought-iron crucibles, when strongly prepared and carefully made, will stand about thirty of these fusions, giving way in the end on account of the action of the sulphur contained in the ores.

    [Illustration: Fig. 4. Iron Casting-moulds.]

    Another kind of crucible, in addition to those already mentioned, is used by the trade, and is recommended by many assayers as superior to all others. Fig. 6 represents the form of it. It is about 4-1/2 ins. high, and 2 ins. in its greatest interior diameter, being in the form of a skittle. The charge consists of the following in this assay:

    Finely powdered ore 60 grains.
    Small pieces of iron 12 "
    Black flux 180 "
    Common salt 50 "

    Put the powdered ore into the crucible, and place upon it the iron, which should not be in the form of filings or dust, but in small pieces; upon the ore and iron should be put the black flux, and lastly the common salt must be placed above all these substances as a protection against the air. The crucibles, as many as convenient, may now be introduced into the furnace, and slowly raised to a strong red heat, at which temperature they should be kept for about half an hour; at the end of that period they should be removed from the fire, slightly tapped to settle the contents, and then placed aside to cool.

    When this has taken place, a few blows with a hammer near the base of the crucibles, each in turn, will soon expose the button of silver attached to the undecomposed iron; the latter substance may, however, be easily detached by a few well-directed blows with the hammer.

    [Illustration: Fig. 5. Iron Crucible for Assay.]

    [Illustration: Fig. 6. Fire-clay Crucible for Assay.]

    In order to ascertain the exact amount of the precious metal--that is, the silver--contained in the buttons of lead obtained as the results of the foregoing operations, they are subjected to a purifying process by the metallurgist, called cupellation. By this means the lead and other impurities are driven off by heat in contact with a current of air, and the silver is left behind in a pure state. To perform this operation it is necessary to expose the buttons on some absorbing medium or porous support, and this support is commonly known as a cupel.

    No doubt many porous substances could be made available for the formation of cupels, but bone-ash is the best for all practical purposes, such as are required by the assayer. The bone-ash, in the condition of a very fine powder, is mixed with a little water in which has been dissolved a small quantity of potash, and moulded into the desired shape. The cupels are tightly consolidated by pressure in an iron mould of the form shown in Fig. 7, which is the best in use, being well adapted for the manufacture of cupels.

    It consists of a slightly conical steel ring, 2 ins. in depth, and about 1-1/2 in. in diameter at the top internally; a steel die with a wooden handle (Fig. 8) is made to fit the mould. To make a cupel the space in the ring is nearly filled with the moistened bone-ash, and pressed down by the hand, and afterwards by the die, the latter being driven into the ring by the application of a wooden mallet (Fig. 9) to the handle of the die.

    It will be seen from the illustration that the die forms a cavity in the cupel capable of receiving the charge of metal for assay. When the bone-ash has been sufficiently compressed, the die is withdrawn, and the cupel removed from the ring. This is a delicate operation, as sometimes the edges of the cupel are liable to be injured; to prevent which and facilitate the removal a loose plate of iron, exactly fitting the bottom of the mould, should be introduced previous to putting in the bone-ash.

    The iron plate of course being removed with the cupel, it must be replaced before another can be made. By introducing a cylindrical piece of wood to the lower aperture of the steel ring, the cupel can be removed without difficulty.

    [Illustration: Fig. 7. Cupel Mould.]

    [Illustration: Fig. 8. Die for Cupel.]

    [Illustration: Fig. 9. Wooden Mallet.]

    The size of the cupel should always be regulated according to the quantity of foreign matter to be absorbed, it being generally understood that the material of which it is formed takes up double its weight of lead. The process of cupelling is conducted in the furnace of the assayer, an apparatus of peculiar construction, the most important part of which, however, is the muffle (Fig. 10), consisting of a small arched oven of fire-clay closed at one end, and furnished with perpendicular slits in the sides, in order to allow of a free access of air to the cupels inside.

    [Illustration: Fig. 10. Assayer's Muffle for Cupels.]

    [Illustration: Fig. 11. Cupel Tongs.]

    [Illustration: Fig. 12. Cupels, section and perspective views.]

    The position of the muffle in the furnace is so arranged that it can be readily heated on every side; and when it has become red hot, six or eight cupels, previously well dried, are taken and placed on the floor of it, which should be covered with a thin layer of bone-ash.

    The form of tongs required for this purpose is shown in Fig. 11. When the cupels have been raised to the temperature of the muffle itself, the assays are put in by a very slender pair of tongs, the door of the furnace is then closed for a few minutes, when the metal will have become fused, and the litharge will begin to be taken up by the bone-ash of which the cupel is composed. The temperature of the furnace is now lowered as much as possible, although not to such an extent that it will retard the progress of oxidation and absorption.

    When nearly the whole of the lead has been thus absorbed, the bead remaining will have become very rich in silver, and, as the oxidation proceeds, will appear much agitated, assuming a rapid circular movement, and revolving with great rapidity. The silver gradually concentrates itself in the centre of the cupel, taking the form of a globule, and at this stage the fire should be made sharper, the operation being carefully watched.

    When the last particle of lead leaves the silver, the agitation will suddenly cease, and a beautiful phenomenon be witnessed, called by assayers the brightening. The button of silver then becomes brilliant and immovable, and the operation, when this takes place, is complete.

    The cupel must be cooled with very great care, in order to prevent the silver from sprouting; which if allowed to take place would result in considerable loss, besides destroying the accuracy of the assay.

    To prevent this sprouting it is a good plan immediately to cover the cupel by another, which has been heated for that purpose; the two are withdrawn together, and allowed to remain at the mouth of the muffle until the silver has become solid; the metal is then in a state of almost chemical purity, and may be detached and weighed. Previous to the latter, however, it should be carefully cleansed from all foreign matter, and flattened on a smooth-faced anvil, this process greatly assisting in the removal of any oxide of lead, which not unfrequently attaches itself to the globule of silver.

    The weighing is conducted with a pair of scales having an extremely delicate balance; and where any commercial transaction depends upon the accuracy of the assay, it is always imperative to make several tests of the same sample, to avoid the consequences of any accident or mistake.

    The chief element in combination with silver on the large scale is lead. Formerly the plan adopted in the separation of this metal was cupellation alone. This process on the large scale is somewhat different from that just described; and as it may appear to the reader interesting and instructive, a brief explanation of it may not be considered out of place.

    CHAPTER IV.

    The Cupellation of Silver Ores.

    This interesting process is performed in a reverberatory furnace of a very peculiar construction, the cupel employed on the large scale differing somewhat from the ordinary one, being considerably larger and varying also in form. It consists of a strong oval wrought-iron ring, with a part of the full shape omitted, as shown in accompanying sketch, in order to allow of the overflow of lead during the process, in the form of litharge.

    This iron ring, known as the test ring, contains the cupel, and in order to prepare the latter, the frame, which measures about 60 ins. in its longest diameter, 40 ins. in breadth, and 6 ins. in depth, is strengthened by having a number of broad strips of iron seamed across the bottom by riveting to the sides of it.

    The cupel itself is prepared for use by taking finely ground bone-ash, together with a little carbonate of potash, and working them up with just sufficient water to make the mass cohere properly; the carbonate of potash may be advantageously dissolved in the water; the latter is then applied in small quantities at a time to the bone-ash until the proper coherency has been obtained; of the total quantity of bone-ash employed in the operation, 2 per cent. of potash will be quantum sufficit to mix with it.

    The iron frame, or test, is then filled with the mixture, and it is pressed down into a solid compact mass, the centre part being hollowed out with a small trowel, the sides sloping towards the concavity in the middle; the hollow should not however be extended more than within 1 to 1-1/2 in. of the bottom of the frame, and above the iron bars. The cupel forms the hearth of the furnace we have spoken of, and of which Fig. 13 is a sectional view; it is removable, and not a fixture in the furnace.

    It must be left for several days to dry, after having been constructed as described, when it is ready for use, and only requires firmly wedging in its place beneath the arch of the furnace.

    [Illustration: Fig. 13. Cupels, section and perspective views.]

    The fire should be only very moderate at the commencement of the operation, and the furnace slowly raised in temperature, lest the cupel should crack by being too quickly heated.

    As the temperature increases, if without any apparent defects in the bone-ash cupel, or hearth, which it may now be termed, the wind or blast, generally driven by a fan, is thrown in through a nozzle, or an aperture in the furnace, which, for facilitating the immediate removal of the bone-ash hearth, is placed upon an iron car, and runs beneath the vault of the furnace on rails, so that it may thus be very readily withdrawn when found necessary.

    The admission of a current of air into the furnace oxidizes the excess of lead, in combination with the silver, producing litharge on the surface of the molten mass; the formation of the litharge takes place rapidly, and it is continually blown forward by the strength of the blast as fast as it is produced, running through a gap or channel specially made for the purpose in the mouth of the cupel into a movable iron pot which is placed for its reception.

    The continual oxidization and flow-off of the lead alters the respective proportions of the metals in the cupel.

    For this reason it is always kept full of lead ore, which is effected by taking it in its fused state from a kettle in which it is ready melted by means of a long-handled ladle; and thus about 500 or 600 lbs. of metal are constantly kept in this bone-ash cupel or hearth.

    As the silver necessarily increases in the hearth, it will require to be occasionally withdrawn, in order to make room for a further supply of lead ore. This process is adopted when it reaches about from 8 to 10 per cent. of silver to the ton (between 2,000 and 3,000 ozs.), and may be effectually performed by drilling a hole underneath the cupel, and letting the silver flow through it into a receptacle placed to receive it. Of course the operations of the furnace are arrested while these manipulations are being carried on.

    After the withdrawal of the silver, the hole is closed up again with a plug of moistened bone-ash prepared as before; when the process may be continued a second time by giving 500 or 600 lbs. of fresh lead ore to the cupel. Thus a single cupel will often last 48 hours, and 6 or 7 tons of lead may be oxidized upon it.

    We have already observed that the prolongation of the cupelling process increases the richness of the remaining alloy, and this very rich silver-lead alloy is again subjected to a second operation in cupelling.

    This process of assaying or refining is similar in every respect to the former, and is often performed in the same furnace, the cupel being first of all brought to almost a bright red heat, when about 600 lbs. of the silver-lead alloy are added, and a strong current of air given in order to oxidize the remaining lead in combination with the silver. In this operation the material under treatment, previous to its introduction to the cupel, should be melted in a kettle easy of access, and added in its fused state.

    The current of air in connection with the heat of the furnace immediately begins to purify the silver by oxidizing the lead, and forms litharge, which passes off through the channel provided in the mouth of the cupel; as this proceeds, fresh silver-lead alloy is added, to keep the level of the metal always at the same height. This is continued until some three tons of the alloy from the first cupellation have been put in, and when about 600 or 700 lbs. of silver are collected in the cupel.

    When the cupel has received the above proportion of metal, the addition of the alloy ceases, and the silver is allowed to purify. The litharge which passes off towards the close of this process will be richer in silver than in the former one; consequently it is found best in practical metallurgical operations to treat in a special manner the last part of silver cupelling on the large scale, for it needs very careful management indeed to secure all the silver, especially to do so in a fine state.

    Towards the completion of the process the fire should be increased considerably, in order to keep the silver thoroughly melted, and also to oxidize and completely remove every trace of lead that is possible. As it begins to purify itself from the remaining lead a characteristic brightness will be perceived. When this takes place the fire must be lowered, the wind or blast stopped, and the metal left to cool gradually.

    This latter proceeding is of some importance, as a too sudden cooling of the surface causes the interior of the metal to expand and shoot, by which means little globules of silver may be lost; therefore it should be allowed to cool very slowly.

    The iron ring encircling the cupel with its contents may now be drawn from beneath the arch of the furnace, and the cake of silver taken from its bed in the bone-ash which formed the vessel, and cleaned of any impurity; when it may be re-melted in a plumbago crucible, and cast into ingot moulds. These moulds should be made of iron, and should always, when used for this purpose, be warmed and greased a little, previous to the introduction of the melted material, to prevent the metal from spitting and adhering to it.

    If skilfully treated during the process of cupellation, the desilvered lead seldom contains more than ·002 to ·003 per cent. of silver to the test assay of 200 grs., or between six and ten pennyweights to the ton, beyond which point it is unprofitable to carry on the operation.

    The litharge which is formed and passes off during the process gradually grows richer in silver towards the end of the cupellation. It probably contains after concentration about thirty to forty ounces of silver to the ton of litharge. This is again subjected to the several operations of the same kind for the recovery of the silver.

    It is somewhat remarkable that the present method of recovering and purifying this metal bears a strong resemblance to that employed in ancient times, and which is spoken of in the Holy Scriptures by the prophet Ezekiel (xxii.

    18 and 20): "Son of man, the house of Israel is to me become dross: all they are brass, and tin, and iron, and lead, in the midst of the furnace; they are even the dross of silver." And also, "As they gather silver, and brass, and iron, and lead, and tin, into the midst of the furnace, to blow the fire upon it, to melt it; so will I gather you in mine anger and in my fury, and I will leave you there, and melt you." The celebrated metallurgist Dr.

    Lamborn says, "Only those who have seen, beneath the glowing arch at the smelting works, flames surging wave after wave across the surface of the liquid metal, carrying all the substances, here called dross, from the pure silver; and only those who have heard the roar of the fiery blast, that ceases neither day nor night, until its task of purification is accomplished,--can appreciate the terrible force of the figure made use of by the prophet." According to the above scriptural passage it is evident that the ancients were in possession of the first rudiments of assaying, and understood to some extent the purification of metals; but scriptural testimony does not point out with what amount of skill and success these operations were performed.

    Judging from the appliances which have been handed down from generation to generation, we are inclined to think they must have been practised somewhat rudely; for it has been left to the present school of scientific and practical metallurgists to found and develop the art in the direction of that commercial success to which it has at the present day attained.

    This plan of cupellation which we have just described is still adopted in many continental works in the assaying of silver-lead ores. In England the system has been almost entirely superseded by one invented by the late Mr. Pattinson of Newcastle, and which is confidently stated to be far more convenient in practice.

    CHAPTER V.

    The Alloys of Silver.

    Fine silver enters freely into combination with nearly all the useful metals, but its most important alloys are those prepared from copper, the latter substance being more suitable for the production of silversmith's work than any other; whilst it produces a more pleasing effect, if not over-alloyed, in regard to finish. Silver articles, especially of the filigree kinds, if the designs are good, possess a very tasteful appearance.

    In treating of the alloys of silver, it is our intention, first, to give a cursory glance at the chemical and physical properties of the metals which form these alloys. Such a description, although brief, will, we believe, prove of essential service, not only to working silversmiths and metalsmiths, but also to goldsmiths and jewellers, who are constantly manipulating with these inferior metals in precisely the same way as the silversmith.

    Besides, such information cannot, we apprehend, fail to be useful, whether to the student, the theorist, or the practical worker.

    An alloy is the union of two or more metals by fusion, so as to form a metallic compound. It may consist of any number of the metallic elements, and in any proportion, provided they will chemically combine, always excepting mercury as one of the ingredients. In this latter case the mixture is called an amalgam. Chemistry has made us acquainted with about forty-nine metals; of that number, however, not more than fourteen are employed to any considerable extent for industrial art purposes.

    They are as follow: Gold, silver, copper, zinc, platinum, aluminum, nickel, iron, mercury, lead, tin, arsenic, antimony, and bismuth. Some of these are occasionally employed for special purposes in the arts in their pure state; but where hardness is to be a distinguishing characteristic, combined with certain variations in shades of colour, a union is effected of two or more of these metals in different proportions, by fusion and stirring, so as to form the requisite alloy.

    Metals used in the pure state, that is, without any mixture of alloy, have very few applications in regard to industrial pursuits and the arts. The precious metals--gold, silver, &c.--would be much too soft, while, on the other hand, arsenic, bismuth, and antimony would be far too brittle to be employed alone for manufacturing purposes. It is quite possible to effect some thousands of alloys, but there do not appear to have been more than about three hundred practised successfully for commercial purposes.

    The principal alloy of silver, as we have already remarked, is copper; but, occasionally, nickel, and even zinc are employed in the case of the commoner qualities of silver. Tin is also used in the preparation of solder for these qualities, in order to render it the more easy of fusion when used for soldering the work. Of the distinctive features of these elements of silver-alloy we shall now speak with some amount of detail.

    Silver will unite with copper in various proportions by melting the two ingredients together, and stirring them whilst in a fused state. A product will thus be formed differing physically in character from fine silver, caused by the loss of some little of the latter's ductility and malleability; but, on the other hand, a compound will be produced harder and more elastic, which is in every sense better adapted to the manufacture and also to the durability of the articles made by the silversmith.

    Copper, like the precious metals, appears to have been known from a very early age, being one of the six metals spoken of in the Old Testament; and described by the historian as being also one of the seven made use of by the ancient philosopher. It is of a reddish colour, malleable, ductile, and tenacious. It is largely employed in alloying both gold and silver for the manufacture of jewellery and other articles. With regard to malleability, it stands next to gold and silver in the list of useful metals; in ductility it occupies the fifth position; and in tenacity one only is superior, viz. iron.

    It is not very fixed in the fire, for if subjected to a long-continued heat it loses a part of its substance; for this reason the alloys of silver and copper should be carefully watched in the crucible to prevent this loss when under the action of the fire.

    When struck copper gives only a feeble sound, and is easily abraded by the file. It fuses at a good white heat, or about 1994° Fahr., although some authors have given it as 1996° Fahr. Its specific gravity varies between 8·88 for cast copper, and 8·96 when rolled and hammered. It loses between one-eighth and one-ninth, or 4/35ths, of its weight in water.

    When exposed to a damp atmosphere a greenish oxide, called verdigris, is produced on its surface, and this is one of the reasons why silver articles containing a percentage of copper become so readily discoloured if left exposed to atmospheric influences; copper also, if heated in contact with the air, quickly becomes oxidized, and, on being touched, scales fall off: these form the protoxide of copper.

    If this process is frequently repeated under a great heat, each time the metal is operated upon it loses a part of its malleability and ductility, which are both eminent characteristics of the pure metal. Most of the ordinary acids act on copper but slowly in the cold, but nitric acid very readily dissolves it, even if largely diluted. Copper amalgamates with most of the metals, and its subsidiary alloys are very largely employed in the arts and manufactures of every kind.

    The bean-shot copper of commerce, costing about a shilling per pound avoirdupois weight, is quite good enough for all the practical purposes of the silversmith.

    [Illustration: Fig. 14. Venus. Egyptian Mark for Copper.]

    The name given to this metal by the alchemists was Venus (Fig. 14), which is one of the principal planets, whose orbit is situated between the Earth and Mercury. The scientific name of cuprum for copper is derived from the Isle of Cyprus, where, it is said by Pliny, the Greeks discovered the method of mining and working it. Copper is found distributed all over the world; a considerable portion, however, is found in the United Kingdom.

    Nickel.--This metal is found chiefly in the Hartz Mountains. It was formerly called by the Germans "Kupfer nickel," or false copper, "nickel" being a term of detraction. It was first discovered about a century and a half ago by Cronstedt. It has a greyish-white colour, and is slightly magnetic, i.e. it is attracted by the magnet in the same way as iron and steel, but it loses this property if heated to about 600° Fahr. Its specific gravity varies between 8·40 and 8·50, according to the amount of compression it has received, and it is rather brittle; it may, however, be drawn into wire, and rolled flat, or into sheets.

    It is considerably harder and less ductile than any of the other metals employed in jeweller's and silversmith's work. In hardness it nearly approaches iron, and on this account, when polished, a characteristic brightness is produced. The malleability of nickel is less than that of iron, standing tenth in the list of useful metals; and in ductility it also occupies the tenth position. Nickel is very infusible, and does not so easily oxidize or tarnish at ordinary temperatures as copper does. Several countries have tried to employ it in the manufacture of small coin for the currency, but its use has now been almost abandoned.

    Nickel alloys are much used in the arts for manufacturing purposes, under the name of "German silver," there being large demand for this metal, as it forms the hard white alloy much used in making "electro-plate," and on which silver is afterwards deposited. It also is used in common silver alloys, in order to keep up the whiteness of the latter element, the addition of too large a proportion of copper maintaining the tint of the latter metal, in too strong a degree to be altogether employed by the silver-worker.

    Nickel is sometimes specially employed, in combination with other metals, to replace or imitate silver in the manufacture of commercial wares, while with copper, zinc, tin, &c., it forms very useful alloys, producing great hardness.

    Zinc.--This metal in its pure state is sometimes called spelter. At the present day it is not much used for alloying silver; but, as it is commonly employed in the preparation of silver-solder, it is necessary that the amateur and the student should know, as well as the practical mechanic, the distinctive characteristics of it, together with the qualities it imparts to others when in combination with them.

    As a metallic substance it was unknown until a long time subsequent to the discovery of the principal metals; and only since the commencement of the present century has its uses been thoroughly known and appreciated in the industrial world. In its pure state, zinc is a bluish-white metal, hard and highly crystalline; but, when raised to a heat of between 250° and 300° Fahr., it is malleable, and may safely be rolled and hammered: it is in this way that the zinc of commerce is produced.

    Zinc may be annealed by placing it for a time in boiling water.

    Its specific gravity varies between 6·8 and 7·2, according to the previous kind of mechanical treatment it has received. At 773° Fahr. it melts, and is quickly oxidized by exposure to a current of air, emitting white vapours, which rise into the air, and are not unlike cotton-flakes; oxide of zinc is thus formed by the burning away of the zinc.

    Spelter or zinc is employed by jewellers in the manufacture of bright gold alloys, as it gives liveliness of colour to their wares not to be equalled by any other metal. (For the proportions and treatment of this composition see "The Goldsmith's Handbook.") It may be alloyed with most of the metals we have named; its uses in roofing, gutters, spouting, and chimney-pots being all well known.

    All the acids very readily attack it in the gold, and even when largely diluted; it speedily tarnishes, and becomes covered with a white oxide which protects the metal from atmospheric influences. In point of malleability zinc stands eighth among the metals, seventh in ductility, and as regards tenacity about seventh also. In chemistry it is represented by the symbol Zn. Its value when in a state of purity, commercially speaking, is about 4_d._ per. lb.

    Tin.--This appears to have been one of the oldest known metals, and was employed in the Egyptian arts by the ancients, in combination with copper. Its colour is white, with a shining lustre almost as brilliant as that of silver, but it tarnishes much more quickly than alloys of the latter metal. With the exception of aluminum and zinc, it is the lightest of all the metals, its density being between 7·0 and 7·3, whether cast, hammered, or rolled.

    It is found in abundance in Cornwall, where it was also obtained at a very early period by the Ph[oe]nicians; and it is reported in Soame's "Latin Church," p. 30, that it was through the medium of the trade in tin that Christianity was first introduced into this country. Tin is not of a fixed nature like gold or silver, but melts in a moderate fire long before it becomes red hot, or about 442° Fahr.

    It is rapidly oxidized when kept for a long time in a fire having a free access to the air; and it is dissolved by hydrochloric, sulphuric, and nitric acids, the latter acting on it most powerfully. Tin should not be alloyed with gold or silver, as with either of these it easily enters into combination by fusion, rendering them extremely brittle, especially in the case of silver, which becomes by the least mixture of it so brittle that it is totally unfit for the work of the silversmith.

    However, for solder, for filing into dust, it may be advantageously employed to promote a quicker fusion; but even for this it should be avoided where it is possible to do so. The vapours of tin are also permanently injurious in the melting of gold, silver, and their alloys, as they render them very unworkable, and the operator being often at a loss to understand the cause of his misfortune; therefore, in melting silver alloys, it is advisable to avoid as much as possible the introduction of little bits of scrap tin into the furnace.

    If such a thing should happen, however, make the fire once or twice stronger in order that the tin may all be destroyed before the crucible containing the silver alloy is put in.

    [Illustration: Fig. 15. Jupiter. Egyptian mark for Tin.]

    Tin is very malleable, moderately ductile, and tenacious, being fifth on the list for malleability, eighth for ductility, and eighth for tenacity. The Egyptian mark or symbol for tin (sign of "Jupiter") was the same as is represented in Fig. 15, and related to the planet of that name, one remarkable for its brightness. In mythology it is understood as representing the supreme deity of the Greeks and Romans.

    The modern scientific name for tin is Sn. Tin loses over one-seventh, or 4/29ths, of its weight in water from its absolute weight in air. In the next chapter we shall treat of the mixing of silver alloys, &c., and in order to make our information regarding the various metals so employed as complete as possible, we shall conclude this one with the following tables, each of which will no doubt be found useful:--

    Table of Metallic Elements.

    +-----------------------+----------+---------------------+
    | Names of Elements. | Symbols. | Specific Gravities. |
    +-----------------------+----------+---------------------|
    | Platinum | Pt | 21·40 to 21·50 |
    | Gold | Au | 19·25 " 19·50 |
    | Mercury | Hg | 13·56 " 13·59 |
    | Lead | Pb | 11·40 " 11·45 |
    | Silver | Ag | 10·47 " 10·50 |
    | Bismuth | Bi | 9·82 " 9·90 |
    | Copper | Cu | 8·89 " 8·96 |
    | Nickel | Ni | 8·50 " 8·60 |
    | Iron | Fe | 7·77 " 7·80 |
    | Tin | Sn | 7·25 " 7·30 |
    | Zinc | Zn | 6·80 " 7·20 |
    | Antimony | Sb | 6·75 " 6·80 |
    | Arsenic | As | 5·70 " 5·90 |
    | Aluminum | Al | 2·56 " 2·60 |
    +-----------------------+----------+---------------------+

    Melting-points of the Principal Metals.

    +--------------------+--------------+-----------------+
    | Names of Elements. | Fahrenheit. | Centigrade. |
    +--------------------+--------------+-----------------+
    | Platinum | { Infusible, except by the |
    | | { oxyhydrogen blow-pipe. |
    | Cast Iron | 2786° | 1530° |
    | Nickel | 2700° | 1482° |
    | Gold | 2016° | 1102° |
    | Copper | 1994° | 1090° |
    | Silver | 1873° | 1023° |
    | Aluminum | 1300° | 705° |
    | Zinc | 773° | 412° |
    | Lead | 612° | 322° |
    | Bismuth | 497° | 258° |
    | Tin | 442° | 228° |
    | Antimony | Fuses a little below red heat. |
    | Arsenic | Volatilises before it fuses. |
    +--------------------+--------------------------------+

    Physical Properties of the Principal Metals.

    +---------------+------------+-----------------+
    | Malleability. | Ductility. | Tenacity. |
    +---------------+------------+-----------------+
    | Gold | Gold | Iron 549 |
    | Silver | Silver | Copper 302 |
    | Copper | Platinum | Aluminum 300 |
    | Aluminum | Iron | Platinum 274 |
    | Tin | Copper | Silver 187 |
    | Platinum | Aluminum | Gold 150½ |
    | Lead | Zinc | Zinc 109½ |
    | Zinc | Tin | Tin 34½ |
    | Iron | Lead | Lead 27½ |
    | Nickel | Nickel | [B] |
    +---------------+------------+-----------------+

    [B] The above weights were lbs. sustained by 0·787 of a line in diameter, in wires of the various metals.

    CHAPTER VI.[C]

    Various Qualities of Silver.

    [C] See observations on Depreciation of Cost Price of Silver in Preface to Fourth Edition (pp. vii, viii), and the new Table of Cost Prices of Alloys in this Chapter, following the Preface (p. ix).

    The chemical and physical properties of fine silver having been dealt with in a preceding chapter, we shall not refer to them again in detail; but, as we have already observed that it is sometimes employed in its pure state for special purposes, it is desirable that we should point out the uses to which it has been applied, especially those of a mechanical nature. With reference to the latter part of the subject we will now proceed to describe the commercial utility of the metal.

    One of the greatest demands for pure silver--if not the greatest of all--is in the manufacture of fine filigree work, a branch of industry extensively practised on the Continent.

    This kind of silversmith's work was attempted to be revived in this country during the years 1864-5, Birmingham and London being the principal places where the manufacture was carried on; but the success of the undertaking as a staple industry must, at the most, have been only a partial one, for it soon declined, and the trade was thus virtually left, as before, in the hands of our Eastern competitors; most of whom produce splendid specimens of the art of filigree and fine wire-working.

    In India this work is wonderfully performed, and it is truly marvellous to witness the beautiful handiwork of the natives who practise this craft. Their productions are quite the work of the true artist, almost every article representing Nature in some of her various forms, such as flowers, animals, serpents, &c., and these are so skilfully imitated that no one could possibly dispute either the faithfulness of the representation or the ability of the workman.

    This is all the more surprising, because in India the natives have not the modern mechanical appliances which we possess in this country. The jeweller there represents to some extent our travelling tinker, only with this difference, that the travelling tinker in this country is generally an inexperienced and unskilful workman, whereas the Indian, if we are to judge him by his work, must be just the reverse.

    Filigree wire-work is manufactured in Italy, Germany, Norway, and Sweden, and the secret of these countries maintaining the monopoly in this branch of the silversmith's trade is that labour there is cheap; and not in any sense because English workmen cannot make the articles in question. It is owing to this cheapness of labour and the inexpensiveness of living that our Continental competitors can beat us by underselling us in the market; and to no other cause can the production of the foreign cheap article be assigned.

    In India the art of working in silver and gold has long been practised, and so particular are the workmen there about the absolute purity of the metals they use, that they refine them by melting five times, under a very strong blast heat, before commencing the work of manufacture.

    The principal places where these art-manufactures are carried on are in Southern India and at Trichinopoly; and in these districts the delicacy and intricacy of the workmanship are brought to the greatest possible perfection. The articles produced there are all "hand-made," and wrought entirely with a few simple tools, such as a hammer and an anvil (both of which are highly polished and burnished), a few fine pliers, blow-pipes, burnishers, scrapers, a pair of fine dividers, and some delicate scales and weights; these, with a few perforated steel-plates for drawing the wire through, comprise the chief appliances of the travelling native jewellers.

    The process of the work is very simple.

    It is commenced by hammering out the metal upon the anvil, and when it has assumed a certain degree of thinness the dividers are next brought into requisition to mark it into certain widths, which are subsequently cut into strips and drawn into very fine wire through perforated steel-plates, a pair of strong pliers being used for the purpose. The holes in the steel-plates consist of graduated sizes, and by this means the strips of metal are soon considerably reduced; and when the proper thinness has been attained the wire is ready for the exercise of the practical skill and dexterity of the artisan, who produces from it the best filigree work in the world.

    Most of the native jewellers have books containing a variety of designs, but they more commonly work from memory, without any reference to patterns.

    The principal localities where this description of work is produced in the highest perfection are Delhi, Cuttack, and Trichinopoly, in India; and Genoa, Paris, Florence, Malta, Norway, and Sweden. The Indian filigree work is the finest and cheapest in the world. The Maltese manufacture a very good kind, and their crosses are much admired; so also do the Chinese and Japanese, but the manufactures of these latter countries are not so tasteful as those of India, consequently they have not been so highly appreciated. Norway and Sweden produce filigree work of a very light weight; but still their productions in this art will not compare in regard to effect with the finest specimens from India.

    We have said that the silver employed by the filigree worker should be in every case absolutely pure; because, when it is quite fine, it is extremely soft and pliable, so that it will remain in almost any form the artist may choose to work it, without that springiness which is found in all alloyed metals.

    However small might be the amount of alloy contained in the metal, the least admixture of it would produce an elasticity in the wire when pressed into form which would make it unworkable for fine filigree purposes; and in this state it would be the utter bane of the workman, as his progress would be altogether impeded in the production of his work.

    It is of the greatest importance that the spirals, and all the various forms required in filigree working, should remain steadily in their places when pressed into shape, without that rebounding which happens in the case of metals of an elastic nature, and in consequence of which no really first-class work can be performed in connection with this art. For such reasons as these it will be at once palpable even to the ordinary reader that fine silver should always be used in preference to alloyed in the manufacture of filigree work.

    The various ornaments of the filigree kind are commonly enclosed in a rim of plain and somewhat stronger wire, which gives additional strength to each part; and, when put together, tends to compose an article of considerably greater durability. In England these outside rims consist exclusively of sterling or standard silver, whilst all the inner work is of the finer material.

    There are several methods of preparing the wire called "filigree." The oldest and the one almost invariably practised in India consists in the first place in drawing down the wire in a circular form until the very lowest possible thinness has been attained, and frequently annealing it during the process, which is done by heating it to a red heat in a muffle placed upon an iron or copper pan. When this process has been effectually performed the wire is taken (if of the proper degree of thinness) and doubled together; these two fine wires are then twisted into one cord, which should be of the fineness desired.

    The wire requires annealing more than once during the process of twisting, and when it is completed it has a corded appearance, it is then ready for the manufacture of the various articles comprised in this kind of work.

    The old plan of twisting was accomplished in the following manner. One end of the doubled wire being firmly secured in a vice or some other suitable instrument, so as to prevent it from turning round and so prevent the progress of the work, the other end of it was also firmly secured in a small hand machine or vice, which was made to revolve by turning a small handle with the right hand, the machine being held and regulated with the left, in order to keep the wire out at its full length so as to avoid knotting in the various parts of it; it was in this manner that fine filigree wire was in the first instance made.

    The second plan was somewhat different, and in regard to the last part of the process it was certainly a great advantage, especially in the saving of labour, as a greater quantity could be prepared in a much less time than by the old method, that being slow in its progress. Here the lathe was made to supply the place of the small hand machine, the speed of which soon brought about the object in view.

    The flattening of this twisted wire has now commonly come into use, and is effected by passing it through small steel rollers, hardened and polished. The object of this is soon manifest, as the labour-saving process is brought prominently into play: the wire in the first place need not be so finely drawn, and secondly the same filigree surface can be made to appear upon the articles as before, by securing the edges of the wires which show the filigree uppermost; and this is always the case in manipulating with this kind of wire. This method is generally in vogue with most filigree workers.

    A third plan of preparing the material for the manufacture of filigree work is, we believe, due to the ingenuity of a celebrated Birmingham firm, who extensively practised this kind of work some years ago.

    The secret is not now generally known to the trade, therefore a few observations bearing upon it will not be unacceptable to those for whose benefit we are writing. The process is commenced in the same manner as before, in the preparation of the round wire, though this need not be drawn so fine, because by this method we have no twisting.

    When the round wire has arrived at the proper size it is flattened in the manner already explained; and when this is done it should be annealed, but experience will dictate best when this particular process should be carried out. After this latter operation the wire is submitted to the action of very small rollers, and bearing the pattern required in small grooves of various sizes. The pattern takes effect upon the edges of the wires only, and resembles the milled or serrated edges of our coinage, only of course the latter bears no comparison with regard to fineness. Lastly, the wire is again passed through the flattening rollers, and then it is ready to be worked up into the object desired.

    Having gone through the general details of filigree working we shall next direct our attention to the component parts and commercial uses of the English standards, together with those of some other countries. In England there are two silver standards, called respectively the old and the new standards. They are as follows:--

    Fine silver per lb. troy.

    Old Standard, 11 oz. 2 dwts. = 925 millims.
    New Standard, 11 oz. 10 dwts. = 959 millims.

    The older of these appears to have been always the legally recognised standard for the coinage, and also for the manufacture of plate. By a law passed, however, in the reign of William III. (1697) it was raised to 11 oz. 10 dwts. of fine silver in the pound troy weight. The manufacture of silver articles from this standard was soon found to be not so durable as those made under the older one; consequently the silversmiths were permitted by a law passed in the reign of George III. (1819) to manufacture from the former standard of 11 oz.

    2 dwts., the use of the new one being likewise permitted for the benefit of those who chose to avail themselves of it; and to this day it remains an English standard, though hardly ever employed.

    By the Silver Coinage Act (10 Geo. 5), the fineness of the British coinage was reduced on account of the increased price of silver bullion; and the silver coinage now consists of one-half silver, one-half alloy, one troy pound of silver being coined into sixty-six shillings. The copper which composes the alloy in the silver coinage hardens the material employed, and it is found to wear better.

    In order to make the matter as simple as possible, we purpose giving a few practical alloys, as follows:--

    Old standard silver alloy, cost 4_s._ 4_d._ per oz.

    oz. dwts. grs.
    Fine Silver 0 18 12
    Shot Copper 0 1 12
    ----------------
    1 0 0
    ================

    If it is intended that the above alloy should be for Hall-marking, it will be advisable to add a little extra silver to the prepared composition, because fine silver purchased from the refiner or bullion dealer is never absolutely pure, consequently the work will not pass the Hall; or better still alloy as follows:--

    Old standard silver for Hall marking.

    oz. dwts. grs.
    Fine Silver 0 18 14
    Shot Copper 0 1 10
    ----------------
    1 0 0
    ================

    The new standard silver is composed of 38-1/3-40ths of fine silver and 1-2/3-40ths of copper alloy; or millesimal fineness 959 parts of fine silver and 41 parts of copper per 1,000 parts; the remedy being as before 0·004 parts.

    New standard silver alloy, cost 4_s._ 6_d._ per oz.

    oz. dwts. grs.
    Fine Silver 0 19 4
    Shot Copper 0 0 20
    ----------------
    1 0 0
    ================

    New standard silver for Hall marking.

    oz. dwts. grs.
    Fine Silver 0 19 6
    Shot Copper 0 0 18
    ----------------
    1 0 0
    ================

    Quality commonly used in England.

    oz. dwts. grs.
    Fine Silver 0 18 0
    Shot Copper 0 2 0
    ----------------
    1 0 0
    ================

    The qualities of the silver employed by the English silversmiths are invariably below the standard, the duties, assay charges, and loss of time in sending the work to the Hall to be marked acting as a great drawback to the trade in the midst of the keen competition of the present day. Silver chains, brooches, buckles, collarets, &c. are for the most part manufactured from inferior metal. In fact, some manufacturers positively refuse to make Hall-marked goods, on account of the great drawbacks attending the marking.

    The alloys of silver are not calculated on the carat system, like gold, but by certain numbers, or other distinctive features, well understood by the particular firms which trade in silver wares. For our present purpose it will be sufficient to distinguish them by using the numerals, 1, 2, 3, 4, &c.; the alloy nearest approaching sterling or standard we shall call No. 1, and so on downwards until the lowest quality has been reached. We may state that silver does not lose its whiteness if not alloyed below equal quantities of the two metals; however, the alloys used in manufactures seldom reach so low a limit.

    Silver alloy No. 1, cost 4_s._ 2_d._ per oz.

    oz. dwts. grs.
    Fine Silver 0 18 0
    Shot Copper 0 2 0
    ----------------
    1 0 0
    ================

    Silver alloy No. 1, same as above.

    oz. dwts. grs.
    Fine Silver 1 0 0
    Shot Copper 0 2 6
    ---------------
    1 2 6
    ===============

    Silver alloy No. 2, cost 3_s._ 9_d._ per oz.

    oz. dwts. grs.
    Fine Silver 0 16 0
    Shot Copper 0 4 0
    ----------------
    1 0 0
    ================

    Silver alloy No. 2, same as above.

    oz. dwts. grs.
    Fine Silver 1 0 0
    Shot Copper 0 5 0
    ----------------
    1 5 0
    ================

    Silver alloy No. 3, cost 3_s._ 6_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 15 0
    Shot copper 0 5 0
    ---------------
    1 0 0
    ===============

    Silver alloy No. 3, same as above.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 6 16
    ---------------
    1 6 16
    ===============

    Silver alloy No. 4, cost 3_s._ 3_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 14 0
    Shot copper 0 6 0
    ---------------
    1 0 0
    ===============

    Silver alloy No. 4, same as above.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 8 12
    ----------------
    1 8 12
    ================

    Silver alloy No. 5, cost 3_s._ 2_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 13 12
    Shot copper 0 6 12
    ----------------
    1 0 0
    ================

    Silver alloy No. 5, same as above.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 9 18
    ----------------
    1 9 18
    ================

    Silver alloy No. 6, cost 3_s._ 1_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 13 0
    Shot copper 0 7 0
    ----------------
    1 0 0
    ================

    Silver alloy No. 6, same as above.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 11 0
    ----------------
    1 11 0
    ================

    Silver alloy No. 7, cost 3_s._ per oz.

    oz. dwts. grs.
    Fine silver 0 12 12
    Shot copper 0 7 12
    ----------------
    1 0 0
    ================

    Silver alloy No. 7, same as above.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 12 0
    ----------------
    1 12 0
    ================

    Silver alloy No. 8, cost 2_s._ 10_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 12 0
    Shot copper 0 8 0
    ----------------
    1 0 0
    ================

    Silver alloy No. 8, same as before.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 13 12
    ----------------
    1 13 12
    ================

    The qualities of the silver alloys have been reduced in this list to various values, and the latter ones are as common as it is possible to make them, without a great and perceptible change of colour taking place in the prepared material. But if it be desired to work a still more inferior metal, then another ingredient must enter into its composition, in order to keep up the whiteness of the silver; and this other metal employed is nickel, the alloys with which we shall have occasion to refer to hereafter.

    Suffice it to say, however, that these inferior alloys of silver, prepared with nickel, are not now much employed by silversmiths in their art-manufactures.

    It will be observed that we have recommended the employment of shot copper in the manufacture of silver alloys: we do so for two reasons--first, because it can be purchased at a considerably cheaper rate than can the ordinary forms of copper, costing only one shilling per lb., whilst the ordinary prepared copper for alloying will cost double that amount; and, secondly, if proper attention has been given to the melting and casting process, the workable qualities of the metal will be found everything that could be desired.

    Therefore an excellent material in all respects can be produced by the means suggested at half the cost of alloy. A considerable saving to a large firm might thus be easily effected by its employment.

    In France there are three silver standards--two to be employed by silversmiths, and one for the coinage, as follows:--

    Fine silver per lb. troy.

    Silver ware, 11 oz. 8 dwts. = 950 millims.
    Coinage, 10 oz. 16 dwts. = 900 millims.
    Silver ware, 9 oz. 12 dwts. = 800 millims.

    It will be seen from the above table that pre-war coinage in France did not represent the highest standard, and also that their principal one was inferior to our highest standard.

    French coinage contained 36-40ths of fine silver and 4-40ths of copper alloy, or millesimal fineness 900 parts of fine silver and 100 parts of copper per 1,000 parts of metal; the highest standard for silver wares contains 38-40ths of fine silver and 2-40ths of copper alloy, or millesimal fineness 950 parts of fine silver and 50 parts of copper per 1,000 parts of metal; the lowest French standard for silver wares contains 32-40ths of fine silver and 8-40ths of copper alloy, or millesimal fineness 800 parts of fine silver and 200 parts of copper per 1,000 parts of metal. The remedy is millesimal fineness 0·005.

    French alloy for coinage, 4_s._ 2_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 18 0
    Copper 0 2 0
    -----------
    1 0 0
    ===========

    French alloy for plate, 4_s._ 5_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 19 0
    Copper 0 1 0
    -----------
    1 0 0
    ===========

    French alloy, lowest standard, 3_s._ 9_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 16 0
    Copper 0 4 0
    -----------
    1 0 0
    ===========

    In the preparation of these alloys with French silver it is undesirable to make any addition of fine silver, in order to enable goods manufactured from them to pass the Hall in safety, because the former is assayed before it leaves the bullion dealers, and the bars of metal are marked with their various standards. Such is not the case in England, and refiners' fine metal is sometimes two or three grams under what it is supposed to be; hence the necessity for the further addition of some fine metal as we have already pointed out, when the object in view is to have goods Hall-marked; without which addition it cannot be effected.

    In Germany there are four silver standards--one for the coinage, and three to be employed in the manufacture of silversmiths' wares; and in that country the various standards are severally applied in the production of fine filigree and other artistic work. The fineness of the standards is as follows:--

    Fine silver per lb. troy.

    Silver ware, 11 oz. 8 dwts. = 950 millims.
    Coinage, 10 oz. 16 dwts. = 900 millims.
    Silver ware, 9 oz. 12 dwts. = 800 millims.
    Silver ware, 9 oz. 0 dwts. = 750 millims.

    As regards the alloy to be employed in the manufacture of these various qualities, copper only must be used, all other metals being forbidden.

    These standards represent all home manufactured articles of silver having reference to the standards of that country, as lately appointed by law.

    German pre-war coinage was the same as French and contained 36-40ths of fine silver and 4-40ths of copper, or millesimal fineness 900 parts of fine silver and 100 parts of copper per 1,000 parts of metal. The highest standard of all is used for silver wares, and contains 38-40ths of fine silver and 2-40ths of copper, or millesimal fineness 950 parts of fine silver and 50 parts of copper per 1,000 parts of metal. The next German standard for silver wares contains 32-40ths of fine silver and 8-40ths of copper, or millesimal fineness 800 parts of fine silver and 200 parts of copper per 1,000 parts of metal.

    The commonest German standard employed by the silversmiths of that country contains 30-40ths of fine silver and 10-40ths of copper, or millesimal fineness 750 parts of fine silver and 250 parts of copper per 1,000 parts of metal indicated. Remedy 0·003.

    Silver alloy for the German coinage.

    oz. dwts. grs.
    Fine silver 0 18 0
    Copper 0 2 0
    ---------------
    1 0 0
    ===============

    Alloy for silver wares of the first standard.

    oz. dwts. grs.
    Fine silver 0 19 0
    Copper 0 1 0
    ----------------
    1 0 0
    ================

    Alloy for silver wares of the second standard.

    oz. dwts. grs.
    Fine silver 0 16 0
    Copper 0 4 0
    ----------------
    1 0 0
    ================

    Alloy for silver wares of the third standard.

    oz. dwts. grs.
    Fine silver 0 15 0
    Copper 0 5 0
    -----------------
    1 0 0
    =================

    Silver goods manufactured according to these standards in Germany, which have recently become law, may be alloyed only with copper, and any foreign substance is not allowed to enter into their composition.

    The remedy permitted in the actual fineness of the silver must not be under three thousandths of the standard specified. The goods to be stamped with the number of thousandths and the name of the manufacturer of them, and the correctness to be certified by the firm named. Experts are appointed by the Government to test this correctness, and if the provisions of the law have been justly observed a government guarantee mark is applied to them.

    CHAPTER VII.[D]

    Silver Solders: their Uses and Applications.

    [D] See observations on Depreciation of Cost Price of Silver in Preface to Fourth Edition (pp. vii, viii), and the new Table of Cost Prices of Alloys in this Chapter, following the Preface (p. x).

    Soldering as applied to silversmith's work is an art which requires great care and practice to perform it neatly and properly. It consists in uniting the various pieces of an article together at their junctions, edges, or surfaces, by fusing an alloy specially prepared for the purpose, and which is more fusible than the metal to be soldered. The solder should in every way be well suited to the particular metal to which it is to be applied, and should possess a powerful chemical affinity to it; if this be not the case, strong, clean, and invisible connections cannot be effected, whilst the progress of the work would be considerably retarded.

    This is partly the cause of inferior manufactures, and not, as frequently supposed, the want of skill in the workman.

    The best connections are made when the metal and solder agree as nearly as possible in uniformity, that is, as regards fusibility, hardness, and malleability. Experience has proved, more especially in the case of plain and strong work (or work that has to bear a strain in the course of manufacture), that the soldering is more perfect and more tenacious as the point of fusion of the two metals approaches each other; the solder having a greater tendency to form a more perfect alloy with the metal to which it is applied than under any other conditions.

    The silver or other metal to be operated upon by soldering being partly of a porous nature, the greater the heat required in the fusion of the solder the more closely are the atoms of the two metals brought into direct relationship; thus greater solidity is given to the parts united, and which are then capable of forming the maximum of resistance.

    It is thus obvious that tin should not be employed in forming solders possessing the characteristics we have just described, for being a very fusible metal it greatly increases the fusibility of its alloys; but when very easy solder is required, and this is sometimes the case, especially when zinc has been employed in the preparation of the silver alloy, its addition is a great advantage when it comes to be applied to the work in hand.

    Solders made with tin are not so malleable and tenacious as those prepared without it, as it imparts a brittleness not usually to be found in those regularly employed by silversmiths; for this reason it is advisable to file it into dust, and apply it in that state to the articles in course of manufacture.

    The best solders we have found to be those mixed with a little zinc.

    These may be laminated, rolled or filed into dust; if the latter, it should be finely done, and this is better for every purpose. Too much zinc, however, should not be added under any conditions, as it has a tendency to eat itself away during wear, thus rendering the articles partly useless either for ornamental or domestic purposes earlier than might be anticipated.

    Solders thus prepared also act with some disadvantage to the workman using them, for they possess the property of evaporating or eating away during the process of soldering, leaving behind scarcely anything to indicate their presence; consequently the workman has to keep on repeating the process until the connection is made perfect, which is always done at the expense of a quantity of solder as well as loss to the workman as regards time.

    Solders made from copper and silver only are, generally speaking, too infusible to be applied to all classes of silversmith's work.

    Solders are manufactured of all degrees of hardness; the hardest of all being a preparation of silver and copper in various proportions; the next being a composition of silver, copper, and zinc; and the easiest or most fusible being prepared from silver, copper, and tin, or silver, brass, and tin. Arsenic sometimes enters into the composition of silver solders, for promoting a greater degree of fusion; and we have heard of workmen actually refusing to work with any other solder. The employment of arsenic has, however, a tendency to slightly endanger the health of those persons using it in large quantities; and of late its employment has not been persevered in.

    In applying solder of whatever composition it is of the utmost importance that the edges or parts to be united should be chemically clean; and for the purpose of protecting these parts from the action of the air, and oxidation during the soldering process, they are covered by a suitable flux, which not only prevents oxidation, but has also a tendency to remove any portion of it left on the parts of the metal to be united.

    The flux employed is always borax, and it not only effects the objects just pointed out, but greatly facilitates the flow of the solder into the required places. Silver solder should be silver of a little inferior quality to that about to be worked up. The various degrees of fusibility of the several solders are occasioned by the different proportions of the component parts of the elements which enter into their existence.

    For instance, a solder in which tin forms a component part will flow or fuse much sooner than one in which copper and silver alone enter into composition, or of one wholly composed of copper, silver, and zinc, or of silver and brass; therefore it must be understood that tin is the best metal for increasing the fusibility of silver solders, and for keeping up their whiteness. Nevertheless it should always be used sparingly, and even then drawbacks will present themselves such as we have already alluded to.

    It is our intention to give a list of the various solders which have been usually employed with more or less success, so that the silversmith and the art workman will be enabled to select the one most suitable to the particular branch of his trade; and we contend, from experience in the craft, that success of workmanship mainly depends upon this point.

    Hardest silver solder, cost 3_s._ 9_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 16 0
    Shot copper 0 4 0
    ----------------
    1 0 0
    ================

    Hardest silver solder, same as above.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 5 0
    ----------------
    1 5 0
    ================

    Hard silver solder, cost 3_s._ 6_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 15 0
    Brass 0 5 0
    ----------------
    1 0 0
    ================

    Hard silver solder, same as above.

    oz. dwts. grs.
    Fine silver 1 0 0
    Brass 0 6 16
    ----------------
    1 6 16
    ================

    Easy silver solder, cost 3_s._ 2_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 13 8
    Brass 0 6 16
    -------------
    1 0 0
    =============

    Easy silver solder, same as above.

    oz. dwts. grs.
    Fine silver 1 0 0
    Brass 0 10 0
    ----------------
    1 10 0
    ================

    The silver solders here given are not such as we can confidently recommend to the general silversmith, having proved them to be very unsatisfactory in certain classes of work.

    For example, the first solder, except in the case of plain strong work, would be far too infusible to be generally used by the silversmith; the second, although much more fusible, cannot safely be applied to very fine and delicate wire-work, because the brass in its composition is so uncertain: unless specially prepared by the silversmith, it probably, if purchased from the metal warehouses, contains lead; the latter is injurious, and in process of soldering it burns and eats away, much resembling the application of burnt sawdust to the work.

    No really effective work can be produced when the above symptoms present themselves. The same remarks apply to No. 3, which is the most fusible, and when free from lead or other base metal it may be classed as a tolerably fair common solder.

    In the preparation of the solders to which we are alluding, it is preferable to employ, instead of the brass, a composition consisting of a mixture of copper and zinc, in the proportion of two parts of copper to one part of zinc; the operator then knows of what the solder is composed, and if it should turn out bad he will partly know the cause, and be able to supply a remedy.

    The solders that we have found to answer our purpose best are composed of the following elements. The first is described again as hard solder, but it is not nearly so hard as the one previously described.

    Best hard silver solder, 3_s._ 9_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 16 0
    Shot copper 0 3 12
    Spelter 0 0 12
    -------------
    1 0 0
    =============

    Best hard silver solder, same as above.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 4 9
    Spelter 0 0 15
    -------------
    1 5 0
    =============

    Medium silver solder, 3_s._ 6_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 15 0
    Shot copper 0 4 0
    Spelter 0 1 0
    -------------
    1 0 0
    =============

    Medium silver solder, same as above.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 5 8
    Spelter 0 1 8
    -------------
    1 6 16
    =============

    Easy silver solder, 3_s._ 3_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 14 0
    Shot copper 0 4 12
    Spelter 0 1 12
    -------------
    1 0 0
    =============

    Easy silver solder, same as above.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 6 12
    Spelter 0 2 4
    -------------
    1 8 16
    =============

    Common silver solder, 3_s._ per oz.

    oz. dwts. grs.
    Fine silver 0 12 12
    Shot copper 0 6 0
    Spelter 0 1 12
    -------------
    1 0 0
    =============

    Common silver solder, same as above.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 9 15
    Spelter 0 2 9
    -------------
    1 12 0
    =============

    The whole of the above-named solders will bleach or whiten properly if applied to silver of the suitable quality for such purposes. We have used copper and spelter in our silver solders, because we have found from experience that the fewer number of times a solder is melted the better it is for all purposes. This result of our experience is in direct opposition to those authors who have professed to treat upon this subject, and who can have had but a small amount of real practical knowledge, for it is argued by them that the oftener a solder is melted the more properly does it become mixed, and, consequently, the more fit is it for the workman's use.

    To such arguments we are prepared to give a blank denial, and our reasons for so doing we will state further on in this treatise.

    There are various other silver solders used by silversmiths; some few of which it will be as well perhaps, while we are on the point, to enumerate:--

    Silver solder for enamelling, cost 3_s._ 9_d._ per oz.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 5 0
    -------------
    1 5 0
    =============

    Silver solder for enamelling, cost 3_s._ 2_d._ per oz.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 10 0
    -------------
    1 10 0
    =============

    Easy silver solder for filigree work, cost 3_s._ 9_d._ per oz.

    oz. dwts. grs.
    Fine silver 0 16 0
    Shot copper 0 0 12
    Composition 0 3 12
    -------------
    1 0 0
    =============

    Quick-running silver solder, cost 3_s._ per oz.

    oz. dwts. grs.
    Fine silver 1 0 0
    Composition 0 10 0
    Pure tin 0 2 0
    -------------
    1 12 0
    =============

    Silver solder for chains, cost 3_s._ per oz.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 10 0
    Pure spelter 0 2 0
    -------------
    1 12 0
    =============

    Easy solder for chains, cost 3_s._ per oz.

    oz. dwts. grs.
    Fine silver 1 0 0
    Composition 0 10 0
    Pure spelter 0 2 0
    -------------
    1 12 0
    =============

    Common silver solder, cost 2_s._ 9_d._ per oz.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 12 0
    Pure spelter 0 3 0
    -------------
    1 15 0
    =============

    Common easy solder, cost 2_s._ 9_d._ per oz.

    oz. dwts. grs.
    Fine silver 1 0 0
    Composition 0 12 0
    Pure spelter 0 3 0
    -------------
    1 15 0
    =============

    Silver solder with arsenic, cost 3_s._ 9_d._ per oz.

    oz. dwts. grs.
    Fine silver 1 0 0
    Shot copper 0 3 0
    Yellow Arsenic 0 2 0
    -------------
    1 5 0
    =============

    Silver solder with arsenic, cost 3_s._ 6_d._ per oz.

    oz. dwts. grs.
    Fine silver 1 0 0
    Composition 0 6 0
    Yellow Arsenic 0 1 0
    -------------
    1 7 0
    =============

    Easy silver solder, cost 3_s._ 2_d._ per oz.

    oz. dwts. grs.
    Fine silver 1 0 0
    Composition 0 5 0
    Tinsel 0 5 0
    -------------
    1 10 0
    =============

    Common easy solder, cost 2_s._ 9_d._ per oz.

    oz. dwts. grs.
    Fine silver 1 0 0
    Tinsel 0 10 0
    Arsenic 0 5 0
    -------------
    1 15 0
    =============

    Another common silver solder.

    oz. dwts. grs.
    Fine silver 1 0 0
    Composition 0 15 0
    Arsenic 0 1 6
    -------------
    1 16 6
    =============

    A very common solder.

    oz. dwts. grs.
    Fine silver 1 0 0
    Composition 1 0 0
    White arsenic 1 0 0
    -------------
    3 0 0
    =============

    The solders here given will be found amply sufficient to select from, for every operation of the silversmith, and will answer the several purposes for which they have been described. When tin and arsenic are employed in the composition of solder, either together or separately, they should be withheld until the more infusible metals with which they are to be united have become melted; the tin or tinsel should then be added, and when this is well melted with the mass, fling on the top the arsenic, let it melt, stir it well together, and pour it out quickly into an ingot mould already prepared for its reception.

    When silver and brass, or silver and composition, alone form the component parts of the solder, these metals may be put into the melting-pot together, well fused, stirred, and poured out as before.

    Solders into which volatile metals enter, upon repeated meltings, become hard, brittle, and drossy, and are therefore not so good as when the metal has received only one melting; it is for this reason that we have always preferred to manufacture our solders from metals which have not been melted before, or from those which have gone through the process as few a number of times as possible.

    The mode of soldering gold and silver is as follows: Take the solder and roll it out thin between the flattening rollers, or file it into dust, according to the kind of work in hand. If filed into dust, it is all the better if done very fine; and if reduced to a flat state, which should be tolerably thin, cut it into little bits, or pallions, which may easily be performed with a pair of hand-shears, length-ways and afterwards cross-ways.

    When this is done, take the work which is to be soldered, join it together by means of fine binding-wire (very thin iron wire), or lay it upon the pumice so that the joinings can come close together, and will not be liable to move during the process; wet the joinings with a solution of borax and water, mixed into a thick paste, applying it with a small camel-hair pencil; then lay the bits or pallions of solder upon the parts to be united, and having placed the article upon some suitable object, take your blowing instrument (Fig.

    1. and blow with it, through a gas-jet, a keen flame upon the solder

    in order to melt it; this will render the unification of the parts complete and compact.

    [Illustration: Fig. 16. Blowpipes.]

    [Illustration: Fig. 17. Solder-dish.]

    When filed solder is used, the process of charging the article is rather different from the above. In the latter case the filings are commonly put into a small cup-shaped vessel (Fig. 17), in most cases the bottom of a tea-cup, or some other similar vessel, being used for the purpose; a lump of borax is then taken and rubbed upon a piece of slate, to which a little water is occasionally added during the rubbing; when this solution attains the consistency of cream, it is put into the solder-dish and well mixed with the solder.

    This is then applied to the article to be soldered, by means of a charger, consisting of a piece of round metal wire, flattened at one end, and shaped for the purpose it has to serve. The joinings, when this kind is employed, require no boraxing with the pencil, as described under pallion solder; the borax being intermixed with the solder flushes with it through the joinings to be united, thus rendering any further application unnecessary.

    The process to which we are alluding is called "hard soldering," and cannot be applied to metals of a fusible nature; neither must it be attempted in the case of goods bearing the name of plated, which are put together with soft or pewter solder, similar to that used by tinsmiths and gasfitters.

    If there should be any soft solder about the article, to be soldered by the means we are describing, it would be almost certain to destroy it, the soft solder having such an affinity for entering into combination with metals more infusible than itself when overheated.

    There is an art in soldering greater than some people would believe.

    The heat required is of various degrees, some articles requiring a broad rough flame, others a smooth one, and others again a fine pointed one.

    All these circumstances connected with the process, together with others which we could detail, proving that it is an art only to be acquired by practice, must be considered enough; and we proceed to observe that the skilful jeweller in soldering a large piece of work will direct the flame of the gas jet to all parts of it, until it is tolerably hot, and then return to the spot to be soldered, and by a very dexterous movement of the flame, produced by the blow-pipe, increase the heat at that spot until the solder has flushed and the parts are rendered thoroughly secure.

    So far as some of the work of the silversmith is concerned, the process of soldering is a very delicate operation, and ought not to be undertaken by an unpractised hand.

    The method of preparing solder for filigree work is worthy of a passing notice. It is called by the Germans Lemaille solder. In the first place it is reduced to very fine filings, mixed with burnt borax powdered fine, and in this state it is sprinkled from a spouted grater over the work to be soldered. The English filigree workers commonly use clean filed solder, and by means of the camel-hair pencil apply a solution of borax to the work, and then sprinkle the dry solder upon it from the grater.

    In Vienna a kind of powdered borax is employed, called Streu borax, or sprinkle borax. It is composed of the following ingredients, which should be gently annealed to expel their water of crystallization, the whole well pounded and mixed together, and sprinkled over the parts to be joined from the spouted grater as before:--

    oz. dwts. grs.
    Calcined borax 0 17 12
    Carbonate of soda 0 1 12
    Common salt 0 1 0
    ---------------
    1 0 0
    ===============

    The object of this mixture is to prevent the rising of the solder, and to facilitate its flushing. Too much of it should not, however, be put with solder in the grater at one time, as it is as objectionable as too much borax applied in the ordinary way, but every workman will learn from experience concerning these matters. We have tried this mixture, prepared with filed solder in the ordinary way, and found it advantageous at first; but its greatest drawback is the turning of the solder yellow if not quickly used upon the work after mixing, thus rendering the solder permanently injured. For this reason we have had to abandon its employment in the wet state.

    But, in its dry state, to the silversmith for filigree purposes it is likely to be of advantage.

    It may be remarked that this preparation encumbers the work with a great deal more flux than borax does, and consequently it requires to be more often boiled out during the period of soldering together the component parts. This is effected by boiling in a weak pickle of sulphuric acid and water, composed of the following proportions: one part of acid to thirty parts of water.

    CHAPTER VIII.

    On the Melting of Silver.

    The processes of melting and properly mixing silver with its alloys in a crucible are among the first operations of the silversmith, and are, moreover, of great importance in the production of intimate and homogeneous alloys. In order to effect these, however simple they may appear, various precautions are necessary, and certain principles require carrying out to arrive at the best possible results, otherwise a great loss or waste of material may take place.

    To direct attention to those principles, which from very careful attention to the subject we have found to answer best, will first be our aim, and if we succeed in rendering some little service to our fellow-workers in the craft to which our toil and leisure have been devoted we shall feel highly gratified.

    The weighing of the component metals, the selection of the crucible, the charging of it, and the attention it requires whilst in the furnace are considerations to which we cannot too strongly call attention. The regulations with regard to weighing should be strictly and accurately carried out.

    The best and safest plan is, after the various metals have been separately weighed, to re-weigh them, this time collectively, in order to ascertain whether the total weight corresponds with the previous calculation; if it does, the mixture has been properly prepared. We have known both time and trouble saved by the adoption of this precaution, after mistakes had occurred which could not have been detected until the weighing of the bar of metal had taken place after melting.

    There are various kinds of crucibles manufactured for the use of the precious metal workers. Crucibles were so-called from originally being impressed by the alchemists with the sign of the cross. They are calculated to bear very high temperatures, and consist of English, Hessian, Cornish, Black-lead, and Plumbago. The last two are by far the best; the plumbago, however, being the hardest, and capable of standing the highest temperature, is to be preferred before all others. It will also stand more frequent meltings than any of the rest.

    Such crucibles have been known to withstand the heat of the furnace for upwards of fifty times without giving way. The wear of them is very strong and resisting, as they only gradually become reduced in thickness, so that it is easy to distinguish their unfitness for use. Fluxes act on earthern crucibles, particularly English at a high temperature, whilst nitre and carbonate of soda soon destroy them.

    Fluxes are necessary in most cases of metallic reductions: they protect the metal from the air, and dissolve impurities. They are of several kinds, as follows:--

    Vegetable charcoal.
    Carbonate of potash.
    Carbonate of soda.
    Common salt.
    Sal-ammoniac.
    Sal-enixum.
    Saltpetre.
    Borax.
    Sandiver.
    Yellow soap.
    Black flux.
    White flux.
    Crude tartar.
    Brown potash.
    Sub-carbonate of potash.

    All these fluxes have occasional duties to perform, and are therefore of great service to the metallurgist.

    To prevent the cracking or flying of the crucible, when newly employed, it should, before being charged with the precious metal, be well annealed; that is, heated to redness upon a very slow fire--one that is gradually going down, and in which there is no blaze is to be preferred, because the flame has a tendency, on the introduction of a new crucible, to make it fly to pieces.

    When it has become red hot, if a cold bar of iron be introduced it will soon show whether there are any cracks, and if so the crucible should be rejected; on the contrary, if it withstands this test it may be placed aside until required for use, when it may be employed with perfect safety in the melting of silver and its alloys.

    When copper and silver only form the alloys of the silversmith, they should both be added to the crucible at the commencement of the operation; and it is the best plan to put the copper at the bottom, because it is the most infusible metal. By doing so, it will receive the greatest degree of heat, which in jewellers' furnaces always comes upwards and the higher specific gravity of the silver has a tendency to force that metal downwards; consequently, when the two metals have become fused, upon well stirring--which should be done with an iron stirrer tapered at the point, and previously heated to redness--a perfectly homogeneous mass will be the result.

    When the more fusible metals of which we have spoken are to form the component parts of the mixture, different treatment with regard to them will be required.

    They should not be added at the commencement of the operation, but should be dealt with afterwards, in the following manner:--

    Zinc is one of the more fusible metals, and is sometimes employed by the silversmith in his alloys, for the purpose of imparting a greater degree of whiteness to them, as well as rendering inferior silver more easily bleached or whitened; thus assisting to bring back the natural colour of fine silver to manufactured articles, which have partially lost it by the addition of alloy of some other colour. Zinc, when employed in silver alloys, should be cautiously used, and care should be taken not to add too much to a given quantity of material.

    The solder used with silver-zinc alloys should be far more fusible than that employed with the other alloys. If too much zinc be added in the preparation of these alloys, in the course of the work, particularly in the process of soldering, they have a tendency to sweat, and sometimes to eat the metals into holes around the parts to be united; such alloys, therefore, render this process very difficult to perform, besides entailing more labour in the production of a clean and smooth finish.

    [Illustration: Fig. 18. Plumbago Crucible for melting.]

    In melting an alloy of silver, copper, and zinc, the silver and copper should first be melted in a plumbago crucible of the form shown in Fig. 18, and well stirred together in order that they may become properly mixed. The zinc is sold in flat cakes under the name of spelter, and, when required, is usually cut up with a chisel into pieces of various weights suitable for the object in view. When the copper and silver have become well incorporated, the mixture should be protected from the air by a suitable flux, charcoal being the best for this purpose.

    The most suitable time to add it to the crucible in the furnace is when the metals are just beginning to fuse. This flux covers the whole of the surface of the molten mass, and so prevents the action of the air from destroying some of the baser metal. The charcoal should be perfectly pure and in a finely divided state, for if adulterated with any gritty matter (and sometimes such is the case) a very indifferent working material is produced, the evil results of which show themselves in every stage of manufacture.

    These instructions with regard to melting the more infusible metals having been carried out, the zinc is taken with a long pair of tongs (Fig. 19), and held within the furnace, over the mouth of the crucible, until the temperature has almost reached the melting point, when it should be carefully dropped into the fused mass below, quickly stirred, so that it may become intimately mixed with the other metals, and at once withdrawn from the furnace and poured into a suitable ingot mould (Fig. 20).

    The ingot mould should be clean and smooth inside, slightly greased, and dusted over with fine vegetable charcoal; this latter substance prevents the metal from adhering to the sides of the mould. It is, perhaps, almost unnecessary to state that the ingot mould requires heating to a certain temperature before the melted composition is poured in, otherwise serious spouting takes place, resulting in a great loss of metal. On the other hand, the operator should be cautious not to over-heat it, as the same evil consequences may result.

    [Illustration: Fig. 19. Tongs for Melting.]

    [Illustration: Fig. 20. Ingot Mould.]

    The bar of metal upon cooling should be weighed, and the difference--as most meltings show a little--noted. This is loss, but it will be very little, if the above instructions have been strictly adhered to from the beginning of the operation. With the charcoal flux we have referred to, very nice and clean bars of metal can be produced. This flux is always floating upon the surface of the mixture, and, with a little dexterity in the pouring, it can be prevented from coming out of the crucible with the metal; its proper place is at the end of the pouring.

    When tin is employed, either in alloys or solders, its treatment is similar to that described for zinc; such alloys should not be kept too long in the furnace after they have become fused, as they rapidly become oxidized, especially if brought into contact with the air.

    The waste in silver, and in fact of all alloys, is entirely dependent on the duration of the time of fusion. If it is prolonged after the addition of the fusible metals, the loss is greater in every case, than when once melted. The metals should be subjected to the beat of the furnace for the shortest possible period.

    The alloys of silver with zinc would lose more than the alloys of silver with tin, because zinc rapidly volatilises when heated above the temperature of its fusion, and this is especially the case when it enters into combination with silver and copper in the fused state; its vapours can be seen to rise and burn in the air, producing light and white flaky fumes, and, chemically speaking, forming the protoxide of zinc.

    With care and manipulative skill during the process of fusion, the proportion of waste can be reduced to a minimum; and when this is exactly ascertained an allowance can be made in the preparation of the mixture for the crucible. From the above remarks it will be apparent that when both tin and zinc form component parts of a mixture, either to be used as an alloy or as solder, the tin should be added to the other metals, and well stirred, so as to obtain an intimate mixture, before the addition is made of the zinc.

    Scrap silver should be carefully sorted before undergoing the process of re-melting, and if possible all foreign substances removed. It may, if preferred to work it in that way, be melted into a separate bar, or otherwise used as an addition to a new mixture. When, however, it is separately melted, a flux, such as carbonate of soda, may be employed, on account of its cheapness, in small proportions to the charcoal flux already alluded to. In brittle and troublesome alloys we have found charcoal and a small quantity of borax extremely effective.

    Saltpetre is a very useful flux in dissolving impurities, but in some alloys its presence is injurious. Sandiver will remove iron or steel from the mixture. Corrosive sublimate destroys lead and tin. We have found the sub-carbonate of potash one of the best fluxes for silver, when matters have not been quite so straight as they should be in the working of the metal; it is used in melting the difficult alloy of 18-carat gold, and is considered a secret not generally known to the trade.

    Sal-ammoniac is an excellent flux for producing clean and bright ingots and tough alloys. We invariably use it with all our alloys, mixed in small quantities with charcoal, and prefer it to all others.

    Lemel, that is the filings and turnings produced during the process of manufacture, should have quite a separate method of treatment. It is best prepared for the crucible by passing it through a fine sieve, afterwards thoroughly burning it in an iron ladle, and then intimately mixing it with a flux of the following nature and proportions:--

    Silver dust 24 parts
    Carbonate of soda 4 "
    Common salt 2 "
    Sal-enixum 1 "
    ----------
    31 parts.
    ==========

    [Illustration: Fig. 21. Fire-clay Crucible for Lemel.]

    The sal-enixum prevents the rising of the mixture in the crucible--which should be of the skittle shape (Fig. 21)--and keeps it from overflowing; it also possesses a refining capacity the same as saltpetre, and is much cheaper.

    The burning of the lemel has a great tendency to destroy all organic matter that would be likely to cause the mixture to overflow during the period of fusion; but if such a thing should be at all likely to take place, the addition of a little dried common salt would remedy the evil, a small quantity of which ought always to be provided for the purpose. The common carbonate of soda is also a cheap and useful flux to the silversmith.

    Five-sixths of the above flux should be well mixed with the stated proportion of lemel, then placed in the pot, and the one-sixth remaining placed upon the top of the mixture, when it may at once be transferred to the furnace. Great heat is required in this operation, and it also requires careful supervision to prevent, if possible, waste of material.

    When the mixture has become perfectly liquid, the heat of the furnace should not be allowed to decrease, but continued for half an hour longer, and if the use of it be not further required, the fire may then be allowed gradually to die out. The mixture will require repeated stirrings during the period of fusion, in order to dissolve such portions as might otherwise not come immediately under the action of the flux.

    When the operation of fusion has been completed, the crucible is withdrawn and allowed to cool, the solidification of the metal is then perfect, and it may be recovered by breaking the pot at the base, when it will fall out in a lump corresponding with the shape of the crucible. The lump of metal should then be carefully weighed, the loss ascertained--which always varies in proportion to the amount of organic matter contained therein; it may then be sold to the refiner, or exchanged for new metal.

    In this process it will be observed that the crucible is broken every time a fusion takes place, consequently some little expense is incurred in providing crucibles for the purpose. To obviate which the following plan may be economically and successfully employed; and especially when the metal is sold to the refiner by assay, the method about to be described will be found most advantageous, for it should be borne in mind that the lump of metal from the previous fusion has to be again run down in another crucible and poured into an ingot mould before the refiner will consent to take his assay from it.

    In this latter process the whole work is performed in one fusion, and the expense of a new crucible thereby saved. The flux employed in the reduction of the metal is also considerably reduced. The plan is performed after the following manner:--

    [Illustration: Fig. 22. Plumbago Crucible for Lemel.]

    Take a plumbago crucible of the shape shown in Fig. 22, and capable of holding the required mixture; put the lemel into it, and then place on the top one ounce of finely powdered carbonate of soda; this is all the flux the mixture requires, and it is then quite ready for the furnace.

    When the lemel has become properly fused, for facilitating which it is repeatedly stirred with a thin iron rod, it is withdrawn and poured into an ingot mould prepared for it as previously described. The flux and other organic matter, which always accumulates upon mixtures of this kind, is held back by the timely application of a thin piece of flat wood to the mouth of the crucible. After the withdrawal of the bar of metal from the ingot mould, it is cooled and weighed, and then it is quite ready for the operations of the refiner.

    CHAPTER IX.

    On the Working of Silver.

    Having reached a most important and very interesting part of our subject, viz. the working of silver, and being desirous of making this treatise useful to the silver-worker in all the branches of his art, it is our intention to enlarge upon these processes--which are purely mechanical--and somewhat minutely to describe the various manipulations and arrangements required in the production of the wares of the silversmith.

    After the removal of the bar of metal from the ingot mould, it should be plunged into a vessel of cold water, dried, and then carefully weighed. At this stage of the process it is ready for the operation of rolling. This process, so far as it concerns large ingots of the metal, is a distinct branch of the trade, and is carried on in separate premises established by certain firms for the purpose. These establishments are called "rolling-mills," the machinery used in them (which is powerful and costly) being moved by steam-power, the reduction of the bars of metal to their various sizes is soon effected.

    The very thin ribbon-shaped metal is produced by submitting it to the action of rollers of smaller dimensions, one after the other, until the desired thinness is obtained.

    The bars of metal are taken to these mills by a man whose special duty it is to watch over them during the processes of rolling and annealing, otherwise it would be very easy to have an ingot of gold or silver exchanged for one of base metal, the mill companies not being responsible for the material intrusted to their care for rolling; hence the necessity for the porter's services, to watch over his employer's interests.

    To prevent accidentally exchanging the bars of metal, through their great similarity to each other, it is the usual thing for the men in charge of them to put a special mark upon the property of each person, previous to the process of annealing. This mark is applied by means of a piece of chalk or soap, and is not removable by heat.

    The annealing is performed in large iron muffles, heated to redness and kept in that condition by flues; the bars which require annealing being placed upon a piece of sheet-iron which slides into the muffle, and there they remain with the doors closed until they have become red hot. It is more particularly during this operation that each person's property requires marking and watching, because of the number of bars admitted at one time into the muffle; and unless the greatest care be exercised at such a time some mistake is almost sure to occur.

    A register is kept of the weight of the metal sent to the mill for the purpose of being rolled into the required shapes and sizes by the manufacturer, who afterwards works it up into different wares and utensils.

    The metal is also weighed on its admittance to the mill, by the clerk of the works, and again on its passage out, and a comparison of the weights registered; but in Birmingham, in some cases, this has been so irregularly performed that great discrepancies have actually taken place in the weights at times, and it has led to the establishment of another rolling-mill for gold and silver, in which the proprietors take upon themselves the whole responsibility and care of metals intrusted to their charge for the above purpose. The method pursued by them in respect to their business is as follows:

    A manufacturer sends a bar of metal to be rolled, carefully noting the exact weight and size to which it is to be reduced upon a proper order head. This weight is carefully tested at the mill, and if found correct, an invoice is given in exchange, upon which is entered the cost of rolling and the time when the work will be completed. The messenger then goes away, returning at the time stated to bring away the rolled metal.

    The advantages this system presents over the others are obvious; the return of the full weight of the metal is guaranteed by responsible persons, the messenger is at liberty during the time occupied in rolling to follow his other duties, the weighing of the respective metals is far more accurately performed both in and out of the mill, besides greater satisfaction being given both to the manufacturer and the roller, the reciprocation of confidence between each, being among some of the additional advantages which might be enumerated. Messrs.

    Kemp, of Birmingham, deserve the thanks of the jewellery community for their enterprising efforts in the establishment of a system so admirably suited to the requirements of the trade.

    The following table gives the charges at the present time for rolling bars of silver:--

    Table of the Cost of Silver Rolling.

    oz. oz. s. d.
    Under 6 0 0 6
    Above 6 and under 12 0 0 9
    " 12 " 18 0 0 10
    " 18 " 25 0 1 0
    " 25 " 35 0 1 3
    " 35 " 45 0 1 6
    " 45 " 55 0 1 9
    " 55 " 70 0 2 0
    " 70 " 85 0 2 3
    " 85 " 100 0 2 6
    " 100 " 115 0 2 9
    " 115 " 130 0 3 0
    Above this 2s.

    6d. per 100 ozs.

    It is a usual thing at all rolling establishments to provide slitting-rolls for those who choose to avail themselves of that mode of cutting up their metal. These rolls are used for the purpose of cutting stout bars of metal into strips suitable for wire-drawing, thus dispensing with the older process of cutting with a pair of vice shears, which method was slow and somewhat uncertain in the production of good work.

    The slitting-rolls consist of circular barrels, after the manner of the "breaking-down" rolls, only of course much smaller in diameter, and with this exception, the slitting-rolls have square grooves cut into each barrel, the projecting portion of each corresponding with the hollow of the other, whereas the breaking-down rolls are perfectly smooth and plain. Rollers something similar to those we have described are used by wire-drawers to facilitate the speedy reduction of the metal, the difference being in the construction and action of the grooves.

    In the grooves of the latter, which are inserted farther apart, the hollows take a half-round shape, and unlike the slitting-rollers, during the revolution of the barrels, the grooves in this case directly meet each other, and thus produce a strip of wire almost round. It is almost needless to remark that wire-rolling requires some amount of practical knowledge to perform it properly.

    The manipulations indispensable to the art of silver working are so varied and so numerous that we are at a comparative loss which part of the process to consider first; however, if we follow the course of the workman with regard to the production of the various manufactures of his art, we shall perhaps not be far wrong in our desire to effect the purpose we have in view.

    In commencing to enlarge upon these mechanical processes we may at once state that it is our intention to refrain from going into the whole art of wire-drawing, because that process has been somewhat minutely alluded to in our other work recently published in the interests of the goldsmiths; the details of which are there fully described.

    [Illustration: Fig. 23. Draw-plate.]

    The draw-plate, Fig. 23, which is the principal tool of the modern wire-drawer, was unknown in this country until the middle of the sixteenth century, when it was introduced by Christopher Schultz, a Saxon, from France. It was supposed to have been the invention of a native of that country named Archal. The draw-plate had been in use some years on the Continent previous to its introduction into England.

    The old method of making wire was upon the anvil, by means of the hammer; and those who manipulated in this art were termed wiresmiths at that period. The best form of draw-plate consists of a piece of steel about nine or ten inches long, one and a quarter to one and a half inch broad, and about half an inch thick, each containing a number of conical holes of various sizes, becoming smaller in succession until the last hole in the plate is reached, when another plate, corresponding in size, having smaller graduated holes, is employed, and the wire drawn through it; and so on, until the proper size has been obtained.

    [Illustration: Fig. 24. Draw-bench for Wire.]

    [Illustration: Fig. 25. Draw-tongs.]

    [Illustration: Fig. 26. Drum used by wire-drawers.]

    [Illustration: Fig. 27. Skeleton Frame or Swift used by wire-drawers.]

    The drawing of stout pieces of wire is effected very readily by means of the draw-bench (Fig. 24), and the thinner pieces, by the application of draw-tongs (Fig. 25), held in the hands of the operator, and made to do service by swinging the body backwards. Very fine wire is now drawn by means of an apparatus called a drum (Fig. 26), revolving upon a perpendicular pin, the exterior of which receives the wire and prevents it from becoming entangled.

    When the end of the wire has finally passed through the draw-plate, the whole coil is carefully removed from the drum (which is made slightly conical in form for facilitating the process) and placed upon a skeleton frame made to receive it (Fig. 27); it is then in proper form for its passage through the next hole of the draw-plate.

    In the production of very fine wire, the metal, after passing a few times through the draw-plate, requires annealing, as its fibres become so condensed and hardened that it is impossible to repeat the operation without some risk of the wire breaking. For fine wire the annealing is repeated five or six times during its passage through the draw-plate; for stouter kinds the annealing need not be so frequent.

    This process produces a scale or oxide upon the surface of the wire, which should be removed before the continuation of the drawing takes place, which is generally done by an immersion for a time in very dilute sulphuric acid pickle; or its passage may be assisted through the draw-plate by the application of some lubricating substance, such as beeswax, or a mixture of beeswax and oil, which enables it the more readily to pass through it.

    In the progress of the wire-drawing the holes have a tendency to become enlarged; these are made smaller again, by repeated blows upon the front of the plate with a somewhat pointed hammer (Fig. 28), and then opened from the back with a tapered steel punch, such as is shown in the woodcut (Fig. 29). The hardening and tempering of the punch is of importance. A gauge-plate is used in all establishments for the purpose of determining the size of the wire.

    The hammering should not take place upon a hardened draw-plate, as it would fly to pieces: it is only those known as soft which should receive such treatment; and those, by a continual alteration of the holes, gradually become hard and require annealing at intervals.

    [Illustration: Fig. 28. Knocking-up Hammer.]

    Draw-plates for wire-drawing purposes are mostly cylindrical in form, but they are employed in various degrees of fineness and in different shapes; such as oval, oblong, half-round, square, fluted, star, sexagon, triangular, and other complex sections, for the production of corresponding wires, all of which receive similar treatment to that above described.

    [Illustration: Fig. 29. Round Steel Punch.]

    The process of wire-drawing, in connection with the art of the silversmith, is more particularly employed in the manufacture of chains, in which branch a very large quantity of silver is consumed.

    This branch of the craft is almost a purely mechanical one, but, nevertheless, there are some designs in chains which require a considerable knowledge of art for the proper execution of them.

    It is, however, in "wrought" or hand-made work that true art is made to play so conspicuous a part; for it is here that perfect workmanship, together with great skill and taste, are required in the manufacture of an article. "Wrought" work was one of the earliest productions of the goldsmith and silversmith, and it still remains the true artistic method, although it has been superseded by others of a less expensive character; such as stamping, chasing, engraving, enamelling, casting, &c., to which the older processes of ornamentation and decoration by means of hammering have given place.

    [Illustration: Fig. 30. Hammer for Wrought Work.]

    [Illustration: Fig. 31. Sparrow-hawk.]

    Wrought work is produced by hammering and soldering the various pieces or ornaments together; and one of the very first things to be attended to in the production of this kind of work is proportion, a knowledge of which is indispensable to true art-workmanship; for the piece of metal which is to be operated upon by the hammer should be of the proper size, so as to require none to be cut off afterwards.

    Every portion of a design should be wrought out of the piece of metal separately, and soldered in its proper place upon the article in process of manufacture.

    When circular forms have to be raised or flanged by the employment of the hammer, as in the case of a raised or flanged brooch "bezil," the modus operandi is as follows:--Take a piece of metal of the exact size and shape, turn the two ends together from the longitudinal direction, and unite them by soldering; when this is done, the circular band of metal is taken and flanged by means of the hammer and a miniature anvil, placed upon a stout piece of wood which the workman renders secure by placing between his knees, the pressure of which retains it steadily in its place during the various manipulations performed upon it; this kind of tool is termed a "sparrow-hawk"--a representation of it is given in Fig.

    31. The work is effected by a series of blows dealt with the hammer in regular concentric circles, the bezil all the time gradually working round the pointed end of the sparrow-hawk. It requires great skill and practice to produce the proper shape, and to keep all parts of the metal of equal thickness.

    The bezils may be produced in this manner round or oval, as well as other complex shapes; the hammering taking place according to the shape required. When raised or ornamental brooch bezils, such as concave or convex patterns, are to be made, the means adopted in their execution are somewhat more complicated than the mode of flanging above alluded to. A tool called a "swage" is employed, which partakes of many forms, the pattern or ornamental device which the metal is required to take being the shape of the swage, or otherwise cut upon it. The metal is easily raised to take the proper design, by a very careful application of the hammering process.

    Sometimes in silver-working the form of the object to be manufactured is of such a nature as not to allow of the use of the swage tool, and this is more particularly the case in the manufacture of plate. Such things, for instance, as cups or tankards which have raised ornamental surfaces, and which have to be executed after the vessel is roughly finished, require altogether a different tool for the effecting of such purposes.

    The one commonly employed in operations of this description consists of a bent piece of steel, upon one end of which is cut the device required; this end being turned up to the required height for raising the design, and the other end being bent in an opposite direction, which, when required for use, is secured in a vice.

    The workman, in executing the design upon the object in hand, places it upon the "snarling-iron" (for such the tool is called) at the part to be raised, and there holds it securely while another man strikes the piece of steel at the top of the angle, or just above where it is secured in the vice, the reaction of the steel wire then throws out the metal, in accordance with the device or pattern cut on the end of it. Designs are only roughly raised in this manner, the perfecting of them being performed by the application of various kinds of chasing tools.

    To prevent a change in the form of the object undergoing this operation, it is filled with a composition formed of pitch, resin, and brick-dust, in the following proportions:--

    Pitch 4 parts.
    Resin 4 "
    Brick-dust 2 "
    ---------
    10 parts.
    =========

    The preparation of the cement is as follows:--Reduce the brick-dust to a very fine powder, and pass it through a fine sieve; then take the other ingredients and melt them in an iron ladle or other suitable vessel over a slow fire, stirring them well together; when this has taken place, the mixture will present a thin liquid appearance, which is the time for using the brick-dust. This should be added in small quantities at a time, and well stirred together, until the mass has become tolerably thick. It is then poured out either upon the floor, or into some suitable vessel provided for its reception.

    While undergoing the operation of chasing, the lower part of the object is preserved from injury, by being laid on a sand-bag. The illustrations, Figs. 32 and 33, represent the snarling-tool, and its mode of application to the work of the silversmith.

    [Illustration: Figs. 32, 33. Snarling-tool, and its mode of application for raising.]

    The progress of the silversmith's art, in conjunction with the researches and discoveries in the mode of working the precious metal during the past century, have wrought a great change both in the style and manner of workmanship. Before the period referred to, the gold and silversmiths' trade was in its lowest possible condition; partly, no doubt, on account of the war then raging on the continent of Europe, and partly because the silversmith at that time was not allowed to manufacture articles of any standard inferior to that of the coinage of 11 ozs. 2 dwts.

    Until the peace of Waterloo, few people were busy but the gun-maker, and other smiths who were able to work at similar occupations; but with respect to most other trades, the men did all they were capable of, in order to earn their daily bread.

    If at that time the silver trade had been specially cultivated, the art, as regards its progress, would have met with many drawbacks, as compared with the present time; the knowledge of the workmen in the production of finished work was not equal to that to be found upon the best articles now manufactured. And although forbidden by law to work in inferior metal, they would have been incapable of effecting the beautiful surfaces which modern articles of inferior quality are made to present.

    The recent scientific discoveries, both chemical and mechanical, that have taken place during the last sixty or seventy years, have wrought a great change in the general conditions, as well as in the mode of the manufacture of silver wares.

    We have said that previous to the year 1815 all was dark and obscure with the precious metal worker, but from that period the work gradually rose in artistic excellence, and the trade very slowly improved; the cause of this no doubt being due, in a great measure, to the security afforded as the result of peace, and with it a revival of the industrial occupations. With the increased industries of the nation arose the pleasures and pastimes of the people, and racing became a national sport.

    This kind of pleasure soon led to an increase in the work of the silversmith, in consequence of the demand for racing cups, which gave opportunities for the artistic excellence of design in their manufacture; and the silversmiths who made them soon acquired a prestige as Art-manufacturers. The demand for work of that and a similar kind led to the employment of regular designers and modellers, who gradually improved both the designs and the work in different parts of the country.

    At the period of which we are speaking, polished or burnished silver goods were most in demand, the modern processes of surface finishing not being then understood. The introduction of the French style of work in filigree soon afterwards caused a demand for that class of work; and the attention of those in the trade was then turned in that direction for a time, and others springing up, the silversmith's and goldsmith's trade generally began to assume a position of importance.

    This kind of work required no polishing and very little artificial finish; besides being exceedingly light in weight and graceful in appearance. It required fine material for its manufacture. In England filigree work has been superseded by other processes, but in India, and in other parts of the East, it is still cultivated to perfection.

    Silver and gold filigree is also manufactured in the Ionian Islands, in Switzerland, and in some parts of Germany and France, where labour is cheap. In the two latter countries it is made from a very inferior material to that used in India. Silver filigree work in this country was soon found not to answer all the requirements of modern society, so far as regarded its utility, durability, and cheapness; fashion therefore demanded something different.

    It is worthy of remark that while this class of jewellery in both gold and silver was so much in vogue for ladies' wear, the old-fashioned seals and keys had undergone a change, and the chasing of them in representation of filigree ornamentation had become the fashion for gentlemen's wear.

    The processes of the manufacture of filigree wire and its mode of application to the work of the artist, have been considered in a previous chapter, further detailed information is therefore rendered unnecessary.

    [Illustration: Fig. 34. Die.]

    When filigree work was no longer used, the fashion changed into "stamped" or "struck-up" ornament. Small pieces of metal were struck-up by means of the hammer and punch, or by the use of the hand-press or stamp; in the former case a lead cake would be prepared, composed of a mixture of lead and tin, and upon it the various ornaments would be produced from the flat metal, corresponding with the pattern of the punch employed for the purpose; in the latter a small die (Fig.

    34) would be employed with the pattern sunk upon it; this would have an aperture through it, the dimensions of the off-side being generally rather large, gradually becoming smaller towards the front surface, which takes the form, in general outline, of the desired pattern. When the necessary blanks have been cut out, another die and punch are used, by which they are raised to their proper shape. These tools should be firmly secured in the press (Fig. 35), otherwise they are likely to be soon destroyed.

    [Illustration: Fig. 35. Press.]

    The small ornaments thus raised were variously arranged one upon another, until a design or pattern was formed, which in every way appeared very showy. Such articles suited the tastes of the people at that time, and still suits those who require good weight for their money. The same kind of thing existed at that period in chains, and being heavy-looking, and costly in appearance, they attracted attention and caused a demand. Thus with the continual changing of the fashions a new era for the goldsmiths and silversmiths of England began.

    They were beginning to work in all sorts of qualities, with the manipulations and finish of which they were becoming now thoroughly conversant, and a demand springing up for goods for purposes of exportation, encouragement was given to the trade, which soon assumed the position of a thriving industry.

    The style of work that followed the "struck-up" patterns was that of plain and solid silver-work, well polished and whitened. This sprung up about the period when coloured gold became the fashion, and the mode of finishing it being somewhat similar, no doubt the demand arose as much from the introduction of colouring as from any other assignable cause. In the chain-maker's branch of the art, a great variety of new patterns came into existence at this period; chain bracelets also began to be introduced; and altogether the trade made rapid strides, and fast rose into a great commercial industry.

    This kind of work has remained more or less in fashion up to the present time, and vast quantities of silver chains of the plain and solid patterns are now being made in Birmingham.

    The silver trade seems to be an exception to the general depression which now prevails in all the other branches of the jewellery trade; the fashion just now is for silver, which causes a greater demand than is usual for goods manufactured of that material.

    In a short time we believe this fashion will undergo a change, and then no doubt manufacturers who have taken advantage of it to make large stocks will have goods remaining upon their hands which they will not be able readily to dispose of, unless at a sacrifice; for it should be borne in mind, that to keep a large stock of silver goods in a saleable condition, and without a quick sale, considerable expense is entailed above the cost of making, to keep them in that condition, through their great liability to become tarnished.

    After the introduction of plain and solid-looking work, it next became the fashion to have it chased over its entire surface. Following this, about the year 1825, came the beautiful process of enamelling, which added artistic beauty to the work, and brought out the harmonies of colour. About this time, too, there sprung up a great demand for the so-called "galvanic ring," which consisted of a lining of zinc and one of silver.

    The ring represented, in appearance, those large, plain, half-round rings which are now made in 18-carat gold, and which weigh from 7 to 10 dwts. each. It was then as now made of half-round shape, and sometimes with the addition of a buckle upon it. The silver was so drawn upon the zinc that the outer surface appeared entirely of silver, and a portion of the inner surface was made to show the zinc only, which was quite sufficient for the purpose required.

    When the ring was put on the finger the zinc, in conjunction with the silver, touched the flesh of the wearer, and was thus supposed to create a galvanic action, which it was alleged had a tendency to remove or prevent rheumatism.

    This kind of work had a good run at the time of its introduction, but like all the rest, the fashion lasted only for a while, when something else had to be brought to the front in the silver trade. The mode of the preparation of the wire was as follows:--A bar of silver would be rolled out until a certain thinness was attained, occasionally annealing it during the process; it was then cut into strips wide enough for the purpose required, again annealed, and subsequently doomed.

    The latter process was effected in this manner:--A block of hard wood, such as boxwood, would be made use of, having a round groove in one side of it, the metal to be doomed would be laid along the groove and a round piece of iron or steel held upon the upper surface with the left hand; a wooden mallet is then taken with the right hand, and by a skilful application of it to the piece of iron or steel, the metal is soon forced down in the groove and made to take the proper form for drawing.

    The flat strip of metal should be pointed; this may either be done before or after the dooming process, though it commonly takes place before. It is performed by taking away a small portion in a conical form, from one of the ends with a pair of hand-shears. A piece of zinc wire should be provided, corresponding in shape with that the ring is to take; this is placed in the hollow of the silver to be drawn, with the flat side outwards, so as to correspond with the aperture in the plate through which it has to be drawn.

    A draw-plate is then taken, with holes of the half-round shape, and the two metals carefully drawn through them. The drawing through a succession of holes produces an edge upon the silver coming against the flat side of the aperture in the draw-plate which overlaps the zinc and thus holds it securely in its place.

    [Illustration: Fig. 36. Hammer for dooming.]

    A change in the style of work gradually took place in the course of every few years, and thus it was that hollow-work became the fashion.

    This kind could be made in a variety of ways, and being very light and showy, it appeared much more expensive than it really was. It is therefore very easy to account for the changes which have taken place in the manufacture of articles of adornment and luxury, and for the encouragement which the art has received.

    With the present styles of the "plain," the "solid," the "filigree," the "stamped," the "mosaic," the "cameo," the "repoussé," the "inlaid," the "enamelled," and a variety of others, we can fearlessly say that silver-working has of late years made rapid progress, and attained to a higher standard than it ever before possessed.

    [Illustration: Fig. 37. Steel Die.]

    [Illustration: Fig. 38. Stamping Press.]

    The art of stamping and shaping articles of jewellery from sheets of the various metals came into general use just previous to the first Exhibition in 1851. These, which are made in considerable numbers, are produced by means of dies, having the shape of the pattern upon them, both at the top and bottom, made of hardened steel. Fig. 37 represents

    Edition notice Project Gutenberg source, credits & licence

    The reading text above is the public-domain work. The Project Gutenberg header, production credits and licence are kept here as provenance rather than shown before the book.

    Title
    The Silversmith's Handbook
    Author
    George E. Gee
    Release date
    December 30, 2014 [eBook #47816]
    Language
    English
    Credits
    Produced by deaurider, Cosmas and the Online Distributed
    Most recently updated
    October 24, 2024
    Transcriber and production notes
    Transcriber Note
    
    Transcriber Note
    
    
    The following changes were made:
    
      p. 47    "Fahr." moved from after "6·8 and 7·2"  =>  to after "773°"
      p. 93    "week pickle"                           =>  "weak pickle"
      p. 175   "regulated workships"                   =>  "regulated workshops"
    
    
    
    
    
    
    End of Project Gutenberg's The Silversmith's Handbook, by George E. Gee
    Front matter as received (title page, contents)
      Emphasized text is displayed as _Italic_.
      Except in tables where the characters ¼ and ½ were used,
        whole and fractional numbers are shown like: 36-1/8.
    
    
    
    
    THE
    
    SILVERSMITH'S HANDBOOK
    
    
    BY THE SAME AUTHOR, UNIFORM WITH THE PRESENT VOLUME.
    
    
    _Ninth Impression, price 5s. net, cloth._
    
    THE GOLDSMITH'S HANDBOOK,
    
    CONTAINING
    
    FULL INSTRUCTIONS FOR THE ALLOYING AND WORKING OF GOLD.
    
     Including the Art of Alloying, Melting, Reducing, Colouring,
     Collecting, and Refining; The Processes of Manipulation, Recovery of
     Waste; Chemical and Physical Properties of Gold; with a New System
     of Mixing its Alloys, Solders, Enamels, and other Useful Rules and
     Recipes.
    
    
    _Crown 8vo, price 3s. 6d. net, cloth._
    
    THE
    
    HALL-MARKING OF JEWELLERY,
    
    PRACTICALLY CONSIDERED.
    
     Comprising an account of all the different Assay Towns of the United
     Kingdom, with the Stamps at present employed; also the Laws relating
     to the Standards and Hall Marks at the various Assay Offices; and a
     variety of Practical Suggestions concerning the Mixing of Standard
     Alloys, and other Useful Information.
    
    
      CROSBY LOCKWOOD & SON,
      7, Stationers' Hall Court, Ludgate Hill, E.C.
    
    
    
    
                                      THE
    
                            SILVERSMITH'S HANDBOOK
    
                                  CONTAINING
    
                               FULL INSTRUCTIONS
    
                                    FOR THE
    
                       _ALLOYING AND WORKING OF SILVER_
    
    
             INCLUDING THE DIFFERENT MODES OF REFINING AND MELTING
             THE METAL; ITS SOLDERS; THE PREPARATION OF IMITATION
                ALLOYS; METHODS OF MANIPULATION; PREVENTION OF
                     WASTE; INSTRUCTIONS FOR IMPROVING AND
                       FINISHING THE SURFACE OF THE WORK
                          TOGETHER WITH OTHER USEFUL
                           INFORMATION AND MEMORANDA
    
                               By GEORGE E. GEE
    
                           GOLDSMITH AND SILVERSMITH
    
    AUTHOR OF "THE GOLDSMITH'S HANDBOOK," "THE HALL-MARKING OF JEWELLERY,"
                                   ETC. ETC.
    
    
                                 Fifth Edition
    
    
                                [Illustration]
    
    
                                    LONDON
                            CROSBY LOCKWOOD AND SON
                    7, STATIONERS' HALL COURT, LUDGATE HILL
                                     1921
    
    
      PRINTED BY
      WILLIAM CLOWES AND SONS, LIMITED,
      LONDON AND BECCLES.
    
    
    
    
    PREFACE.
    
    
    The object of this Treatise is to supply a want long felt in the Silver
    Trade, namely, a work of reference from which workmen, apprentices,
    and manufacturers, employing the material upon which it treats, may
    find information which will be of assistance to them in the performance
    of their daily duties, and by which their operations may be rendered
    more successful. The Author was led to undertake the present work
    from having had many opportunities, during his lengthened experience
    in the art of silver-working, of observing the difficulties and
    stumbling-blocks that are constantly to be met with in the manifold
    branches of this important trade, by those _practically_ engaged in it,
    and also by those persons who are desirous of acquiring a _thorough_
    knowledge of the mechanical and manipulative details belonging to it.
    To assist his object, numerous illustrations have been prepared for
    this Treatise, with the view of rendering the various processes of the
    art more readily comprehensible, and to save a lengthened or detailed
    description of them.
    
    The different modes of alloying and melting silver; its solders; the
    preparation of imitation alloys; methods of working; the prevention
    of waste; instructions for improving and finishing the surface of the
    work, together with other useful information and memoranda--all these
    have been carefully collected and placed in order in the body of the
    work.
    
    The Author has endeavoured, throughout, to present the contents (which
    he has with some little difficulty and labour brought together) in
    as practical and readable a form as is compatible with accuracy and
    efficiency.
    
                                                               G. E. GEE.
    
    
    
    
    PREFACE TO THE SECOND EDITION.
    
    
    Since the publication of the first edition of this work important
    changes have taken place in the commercial value of silver, its
    present cost in the best markets being sixpence per ounce lower than
    it was when this volume first appeared in 1877. This depreciation in
    value has, of course, necessitated a thorough revision of the former
    prices of the various alloys, solders, and other substances mentioned
    throughout the work; and this has been done in order to render it the
    more complete as a work of general reference, conveying correct and
    useful information to the reader. The Author trusts that his endeavours
    in this direction will be appreciated.
    
      58, Tenby St. North, Birmingham.
             _February, 1885_.
    Header as received
    The Project Gutenberg eBook of The Silversmith's Handbook
        
    This eBook is for the use of anyone anywhere in the United States and
    most other parts of the world at no cost and with almost no restrictions
    whatsoever. You may copy it, give it away or re-use it under the terms
    of the Project Gutenberg License included with this eBook or online
    at www.gutenberg.org. If you are not located in the United States,
    you will have to check the laws of the country where you are located
    before using this eBook.
    
    Title: The Silversmith's Handbook
    
    Author: George E. Gee
    
    
            
    Release date: December 30, 2014 [eBook #47816]
                    Most recently updated: October 24, 2024
    
    Language: English
    
    Other information and formats: www.gutenberg.org/ebooks/47816
    
    Credits: Produced by deaurider, Cosmas and the Online Distributed
            Proofreading Team at http://www.pgdp.net (This file was
            produced from images generously made available by The
            Internet Archive)
    Full Project Gutenberg licence
        
    
    Updated editions will replace the previous one—the old editions will
    be renamed.
    
    Creating the works from print editions not protected by U.S. copyright
    law means that no one owns a United States copyright in these works,
    so the Foundation (and you!) can copy and distribute it in the United
    States without permission and without paying copyright
    royalties. Special rules, set forth in the General Terms of Use part
    of this license, apply to copying and distributing Project
    Gutenberg™ electronic works to protect the PROJECT GUTENBERG™
    concept and trademark. Project Gutenberg is a registered trademark,
    and may not be used if you charge for an eBook, except by following
    the terms of the trademark license, including paying royalties for use
    of the Project Gutenberg trademark. If you do not charge anything for
    copies of this eBook, complying with the trademark license is very
    easy. You may use this eBook for nearly any purpose such as creation
    of derivative works, reports, performances and research. Project
    Gutenberg eBooks may be modified and printed and given away—you may
    do practically ANYTHING in the United States with eBooks not protected
    by U.S. copyright law. Redistribution is subject to the trademark
    license, especially commercial redistribution.
    
    
    START: FULL LICENSE
    
    THE FULL PROJECT GUTENBERG™ LICENSE
    
    PLEASE READ THIS BEFORE YOU DISTRIBUTE OR USE THIS WORK
    
    To protect the Project Gutenberg™ mission of promoting the free
    distribution of electronic works, by using or distributing this work
    (or any other work associated in any way with the phrase “Project
    Gutenberg”), you agree to comply with all the terms of the Full
    Project Gutenberg License available with this file or online at
    www.gutenberg.org/license.
    
    Section 1. General Terms of Use and Redistributing Project Gutenberg
    electronic works
    
    1.A. By reading or using any part of this Project Gutenberg
    electronic work, you indicate that you have read, understand, agree to
    and accept all the terms of this license and intellectual property
    (trademark/copyright) agreement. If you do not agree to abide by all
    the terms of this agreement, you must cease using and return or
    destroy all copies of Project Gutenberg electronic works in your
    possession. If you paid a fee for obtaining a copy of or access to a
    Project Gutenberg electronic work and you do not agree to be bound
    by the terms of this agreement, you may obtain a refund from the person
    or entity to whom you paid the fee as set forth in paragraph 1.E.8.
    
    1.B. “Project Gutenberg” is a registered trademark. It may only be
    used on or associated in any way with an electronic work by people who
    agree to be bound by the terms of this agreement. There are a few
    things that you can do with most Project Gutenberg electronic works
    even without complying with the full terms of this agreement. See
    paragraph 1.C below. There are a lot of things you can do with Project
    Gutenberg electronic works if you follow the terms of this
    agreement and help preserve free future access to Project Gutenberg
    electronic works. See paragraph 1.E below.
    
    1.C. The Project Gutenberg Literary Archive Foundation (“the
    Foundation” or PGLAF), owns a compilation copyright in the collection
    of Project Gutenberg electronic works. Nearly all the individual
    works in the collection are in the public domain in the United
    States. If an individual work is unprotected by copyright law in the
    United States and you are located in the United States, we do not
    claim a right to prevent you from copying, distributing, performing,
    displaying or creating derivative works based on the work as long as
    all references to Project Gutenberg are removed. Of course, we hope
    that you will support the Project Gutenberg mission of promoting
    free access to electronic works by freely sharing Project Gutenberg
    works in compliance with the terms of this agreement for keeping the
    Project Gutenberg name associated with the work. You can easily
    comply with the terms of this agreement by keeping this work in the
    same format with its attached full Project Gutenberg License when
    you share it without charge with others.
    
    1.D. The copyright laws of the place where you are located also govern
    what you can do with this work. Copyright laws in most countries are
    in a constant state of change. If you are outside the United States,
    check the laws of your country in addition to the terms of this
    agreement before downloading, copying, displaying, performing,
    distributing or creating derivative works based on this work or any
    other Project Gutenberg work. The Foundation makes no
    representations concerning the copyright status of any work in any
    country other than the United States.
    
    1.E. Unless you have removed all references to Project Gutenberg:
    
    1.E.1. The following sentence, with active links to, or other
    immediate access to, the full Project Gutenberg License must appear
    prominently whenever any copy of a Project Gutenberg work (any work
    on which the phrase “Project Gutenberg” appears, or with which the
    phrase “Project Gutenberg” is associated) is accessed, displayed,
    performed, viewed, copied or distributed:
    
        This eBook is for the use of anyone anywhere in the United States and most
        other parts of the world at no cost and with almost no restrictions
        whatsoever. You may copy it, give it away or re-use it under the terms
        of the Project Gutenberg™ License included with this eBook or online
        at www.gutenberg.org. If you
        are not located in the United States, you will have to check the laws
        of the country where you are located before using this eBook.
      
    1.E.2. If an individual Project Gutenberg electronic work is
    derived from texts not protected by U.S. copyright law (does not
    contain a notice indicating that it is posted with permission of the
    copyright holder), the work can be copied and distributed to anyone in
    the United States without paying any fees or charges. If you are
    redistributing or providing access to a work with the phrase “Project
    Gutenberg” associated with or appearing on the work, you must comply
    either with the requirements of paragraphs 1.E.1 through 1.E.7 or
    obtain permission for the use of the work and the Project Gutenberg
    trademark as set forth in paragraphs 1.E.8 or 1.E.9.
    
    1.E.3. If an individual Project Gutenberg electronic work is posted
    with the permission of the copyright holder, your use and distribution
    must comply with both paragraphs 1.E.1 through 1.E.7 and any
    additional terms imposed by the copyright holder. Additional terms
    will be linked to the Project Gutenberg License for all works
    posted with the permission of the copyright holder found at the
    beginning of this work.
    
    1.E.4. Do not unlink or detach or remove the full Project Gutenberg
    License terms from this work, or any files containing a part of this
    work or any other work associated with Project Gutenberg.
    
    1.E.5. Do not copy, display, perform, distribute or redistribute this
    electronic work, or any part of this electronic work, without
    prominently displaying the sentence set forth in paragraph 1.E.1 with
    active links or immediate access to the full terms of the Project
    Gutenberg License.
    
    1.E.6. You may convert to and distribute this work in any binary,
    compressed, marked up, nonproprietary or proprietary form, including
    any word processing or hypertext form. However, if you provide access
    to or distribute copies of a Project Gutenberg work in a format
    other than “Plain Vanilla ASCII” or other format used in the official
    version posted on the official Project Gutenberg website
    (www.gutenberg.org), you must, at no additional cost, fee or expense
    to the user, provide a copy, a means of exporting a copy, or a means
    of obtaining a copy upon request, of the work in its original “Plain
    Vanilla ASCII” or other form. Any alternate format must include the
    full Project Gutenberg License as specified in paragraph 1.E.1.
    
    1.E.7. Do not charge a fee for access to, viewing, displaying,
    performing, copying or distributing any Project Gutenberg works
    unless you comply with paragraph 1.E.8 or 1.E.9.
    
    1.E.8. You may charge a reasonable fee for copies of or providing
    access to or distributing Project Gutenberg electronic works
    provided that:
    
        • You pay a royalty fee of 20% of the gross profits you derive from
            the use of Project Gutenberg works calculated using the method
            you already use to calculate your applicable taxes. The fee is owed
            to the owner of the Project Gutenberg trademark, but he has
            agreed to donate royalties under this paragraph to the Project
            Gutenberg Literary Archive Foundation. Royalty payments must be paid
            within 60 days following each date on which you prepare (or are
            legally required to prepare) your periodic tax returns. Royalty
            payments should be clearly marked as such and sent to the Project
            Gutenberg Literary Archive Foundation at the address specified in
            Section 4, “Information about donations to the Project Gutenberg
            Literary Archive Foundation.”
        
        • You provide a full refund of any money paid by a user who notifies
            you in writing (or by e-mail) within 30 days of receipt that s/he
            does not agree to the terms of the full Project Gutenberg™
            License. You must require such a user to return or destroy all
            copies of the works possessed in a physical medium and discontinue
            all use of and all access to other copies of Project Gutenberg™
            works.
        
        • You provide, in accordance with paragraph 1.F.3, a full refund of
            any money paid for a work or a replacement copy, if a defect in the
            electronic work is discovered and reported to you within 90 days of
            receipt of the work.
        
        • You comply with all other terms of this agreement for free
            distribution of Project Gutenberg™ works.
        
    
    1.E.9. If you wish to charge a fee or distribute a Project
    Gutenberg™ electronic work or group of works on different terms than
    are set forth in this agreement, you must obtain permission in writing
    from the Project Gutenberg Literary Archive Foundation, the manager of
    the Project Gutenberg™ trademark. Contact the Foundation as set
    forth in Section 3 below.
    
    1.F.
    
    1.F.1. Project Gutenberg volunteers and employees expend considerable
    effort to identify, do copyright research on, transcribe and proofread
    works not protected by U.S. copyright law in creating the Project
    Gutenberg™ collection. Despite these efforts, Project Gutenberg™
    electronic works, and the medium on which they may be stored, may
    contain “Defects,” such as, but not limited to, incomplete, inaccurate
    or corrupt data, transcription errors, a copyright or other
    intellectual property infringement, a defective or damaged disk or
    other medium, a computer virus, or computer codes that damage or
    cannot be read by your equipment.
    
    1.F.2. LIMITED WARRANTY, DISCLAIMER OF DAMAGES - Except for the “Right
    of Replacement or Refund” described in paragraph 1.F.3, the Project
    Gutenberg Literary Archive Foundation, the owner of the Project
    Gutenberg™ trademark, and any other party distributing a Project
    Gutenberg™ electronic work under this agreement, disclaim all
    liability to you for damages, costs and expenses, including legal
    fees. YOU AGREE THAT YOU HAVE NO REMEDIES FOR NEGLIGENCE, STRICT
    LIABILITY, BREACH OF WARRANTY OR BREACH OF CONTRACT EXCEPT THOSE
    PROVIDED IN PARAGRAPH 1.F.3. YOU AGREE THAT THE FOUNDATION, THE
    TRADEMARK OWNER, AND ANY DISTRIBUTOR UNDER THIS AGREEMENT WILL NOT BE
    LIABLE TO YOU FOR ACTUAL, DIRECT, INDIRECT, CONSEQUENTIAL, PUNITIVE OR
    INCIDENTAL DAMAGES EVEN IF YOU GIVE NOTICE OF THE POSSIBILITY OF SUCH
    DAMAGE.
    
    1.F.3. LIMITED RIGHT OF REPLACEMENT OR REFUND - If you discover a
    defect in this electronic work within 90 days of receiving it, you can
    receive a refund of the money (if any) you paid for it by sending a
    written explanation to the person you received the work from. If you
    received the work on a physical medium, you must return the medium
    with your written explanation. The person or entity that provided you
    with the defective work may elect to provide a replacement copy in
    lieu of a refund. If you received the work electronically, the person
    or entity providing it to you may choose to give you a second
    opportunity to receive the work electronically in lieu of a refund. If
    the second copy is also defective, you may demand a refund in writing
    without further opportunities to fix the problem.
    
    1.F.4. Except for the limited right of replacement or refund set forth
    in paragraph 1.F.3, this work is provided to you ‘AS-IS’, WITH NO
    OTHER WARRANTIES OF ANY KIND, EXPRESS OR IMPLIED, INCLUDING BUT NOT
    LIMITED TO WARRANTIES OF MERCHANTABILITY OR FITNESS FOR ANY PURPOSE.
    
    1.F.5. Some states do not allow disclaimers of certain implied
    warranties or the exclusion or limitation of certain types of
    damages. If any disclaimer or limitation set forth in this agreement
    violates the law of the state applicable to this agreement, the
    agreement shall be interpreted to make the maximum disclaimer or
    limitation permitted by the applicable state law. The invalidity or
    unenforceability of any provision of this agreement shall not void the
    remaining provisions.
    
    1.F.6. INDEMNITY - You agree to indemnify and hold the Foundation, the
    trademark owner, any agent or employee of the Foundation, anyone
    providing copies of Project Gutenberg™ electronic works in
    accordance with this agreement, and any volunteers associated with the
    production, promotion and distribution of Project Gutenberg™
    electronic works, harmless from all liability, costs and expenses,
    including legal fees, that arise directly or indirectly from any of
    the following which you do or cause to occur: (a) distribution of this
    or any Project Gutenberg work, (b) alteration, modification, or
    additions or deletions to any Project Gutenberg work, and (c) any
    Defect you cause.
    
    Section 2. Information about the Mission of Project Gutenberg
    
    Project Gutenberg is synonymous with the free distribution of
    electronic works in formats readable by the widest variety of
    computers including obsolete, old, middle-aged and new computers. It
    exists because of the efforts of hundreds of volunteers and donations
    from people in all walks of life.
    
    Volunteers and financial support to provide volunteers with the
    assistance they need are critical to reaching Project Gutenberg’s
    goals and ensuring that the Project Gutenberg collection will
    remain freely available for generations to come. In 2001, the Project
    Gutenberg Literary Archive Foundation was created to provide a secure
    and permanent future for Project Gutenberg and future
    generations. To learn more about the Project Gutenberg Literary
    Archive Foundation and how your efforts and donations can help, see
    Sections 3 and 4 and the Foundation information page at www.gutenberg.org.
    
    Section 3. Information about the Project Gutenberg Literary Archive Foundation
    
    The Project Gutenberg Literary Archive Foundation is a non-profit
    501(c)(3) educational corporation organized under the laws of the
    state of Mississippi and granted tax exempt status by the Internal
    Revenue Service. The Foundation’s EIN or federal tax identification
    number is 64-6221541. Contributions to the Project Gutenberg Literary
    Archive Foundation are tax deductible to the full extent permitted by
    U.S. federal laws and your state’s laws.
    
    The Foundation’s business office is located at 41 Watchung Plaza #516,
    Montclair NJ 07042, USA, +1 (862) 621-9288. Email contact links and up
    to date contact information can be found at the Foundation’s website
    and official page at www.gutenberg.org/contact
    
    Section 4. Information about Donations to the Project Gutenberg
    Literary Archive Foundation
    
    Project Gutenberg™ depends upon and cannot survive without widespread
    public support and donations to carry out its mission of
    increasing the number of public domain and licensed works that can be
    freely distributed in machine-readable form accessible by the widest
    array of equipment including outdated equipment. Many small donations
    ($1 to $5,000) are particularly important to maintaining tax exempt
    status with the IRS.
    
    The Foundation is committed to complying with the laws regulating
    charities and charitable donations in all 50 states of the United
    States. Compliance requirements are not uniform and it takes a
    considerable effort, much paperwork and many fees to meet and keep up
    with these requirements. We do not solicit donations in locations
    where we have not received written confirmation of compliance. To SEND
    DONATIONS or determine the status of compliance for any particular state
    visit www.gutenberg.org/donate.
    
    While we cannot and do not solicit contributions from states where we
    have not met the solicitation requirements, we know of no prohibition
    against accepting unsolicited donations from donors in such states who
    approach us with offers to donate.
    
    International donations are gratefully accepted, but we cannot make
    any statements concerning tax treatment of donations received from
    outside the United States. U.S. laws alone swamp our small staff.
    
    Please check the Project Gutenberg web pages for current donation
    methods and addresses. Donations are accepted in a number of other
    ways including checks, online payments and credit card donations. To
    donate, please visit: www.gutenberg.org/donate.
    
    Section 5. General Information About Project Gutenberg electronic works
    
    Professor Michael S. Hart was the originator of the Project
    Gutenberg concept of a library of electronic works that could be
    freely shared with anyone. For forty years, he produced and
    distributed Project Gutenberg eBooks with only a loose network of
    volunteer support.
    
    Project Gutenberg eBooks are often created from several printed
    editions, all of which are confirmed as not protected by copyright in
    the U.S. unless a copyright notice is included. Thus, we do not
    necessarily keep eBooks in compliance with any particular paper
    edition.
    
    Most people start at our website which has the main PG search
    facility: www.gutenberg.org.
    
    This website includes information about Project Gutenberg,
    including how to make donations to the Project Gutenberg Literary
    Archive Foundation, how to help produce our new eBooks, and how to
    subscribe to our email newsletter to hear about new eBooks.

    Source: Project Gutenberg ebook #47816. Public-domain status is recorded per item; the licence text above is reproduced unchanged.

    Source
    Project Gutenberg
    Record
    ebook 47816
    Rights
    public domain (US)
    Rendered
    2026-11-22
    Completeness
    First 200,000 characters rendered.